*60nm Barc
*60 nm Barc
*360nm KRF resist
*360 nm KRF resist


''by bghe@nanolab'' experiments made in June/July 2012
''by bghe@nanolab'' experiments made in June/July 2012
<gallery caption="Some examples of blazed gratings in fused silica etched with Cr and DUV resist as masking layer "  widths="300px" heights="250px">
<gallery caption="Some examples of blazed gratings in fused silica etched with Cr and DUV resist as masking layer "  widths="300px" heights="250px">


Image:IBE 30min -Cr1.jpg |'''30 min etch with 100nm Cr mask, used recipe BGHE blazed gratings with CHF3''' <br>*Rotation speed 0 rpm<br>*Angle: -35<br>*I(N)=400mA<br>*RF power=1300W<br>*I(B)=300mA<br>*V(B)=300V<br>*V(AC,B)=500V<br>*Ar(N) flow=5sccm<br>*Ar(B) flow=5sccm<br>*CHF3 flow=15sccm
Image:IBE 30min -Cr1.jpg |'''30 min etch with 100nm Cr mask, used recipe BGHE blazed gratings with CHF3''' <br>*Rotation speed 0 rpm<br>*Angle: -35<br>*I(N)=400mA<br>*RF power=1300 W<br>*I(B)=300 mA<br>*V(B)=300V<br>*V(AC,B)=500 V<br>*Ar(N) flow=5sccm<br>*Ar(B) flow=5 sccm<br>*CHF3 flow=15 sccm
Image:after IBE 45min_A_34.jpg |'''45min etch with 100nm Cr mask, used recipe BGHE blazed gratings with CHF3''' <br>*Rotation speed 0 rpm<br>*Angle: -35<br>*I(N)=400mA<br>*RF power=1300W<br>*I(B)=300mA<br>*V(B)=300V<br>*V(AC,B)=500V<br>*Ar(N) flow=5sccm<br>*Ar(B) flow=5sccm<br>*CHF3 flow=15sccm
Image:after IBE 45min_A_34.jpg |'''45min etch with 100nm Cr mask, used recipe BGHE blazed gratings with CHF3''' <br>*Rotation speed 0 rpm<br>*Angle: -35<br>*I(N)=400mA<br>*RF power=1300W<br>*I(B)=300mA<br>*V(B)=300V<br>*V(AC,B)=500V<br>*Ar(N) flow=5sccm<br>*Ar(B) flow=5sccm<br>*CHF3 flow=15sccm
Image:Edge_1.jpg|'''20min etch with Krf resist, all resist is gone, used recipe BGHE blazed gratings''' <br>*Rotation speed 0 rpm<br>*Angle: -35<br>*I(N)=550mA<br>*RF power=1300W<br>*I(B)=500mA<br>*V(B)=600V<br>*V(AC,B)=400V<br>*Ar(N) flow=5sccm<br>*Ar(B) flow=10sccm<br>*CHF3 flow=0sccm
Image:Edge_1.jpg|'''20min etch with Krf resist, all resist is gone, used recipe BGHE blazed gratings''' <br>*Rotation speed 0 rpm<br>*Angle: -35<br>*I(N)=550mA<br>*RF power=1300W<br>*I(B)=500mA<br>*V(B)=600V<br>*V(AC,B)=400V<br>*Ar(N) flow=5sccm<br>*Ar(B) flow=10sccm<br>*CHF3 flow=0sccm

Revision as of 10:23, 4 September 2025

Feedback to this page: click here