Specific Process Knowledge/Thin film deposition/Deposition of Niobium: Difference between revisions
Appearance
mNo edit summary |
|||
| Line 1: | Line 1: | ||
= Deposition of Nb = | |||
Niobium can be deposited by e-beam evaporation or sputtering. In the chart below you can compare the deposition equipment. | Niobium can be deposited by e-beam evaporation or sputtering. In the chart below you can compare the deposition equipment. | ||
Revision as of 14:56, 9 August 2025
Deposition of Nb
Niobium can be deposited by e-beam evaporation or sputtering. In the chart below you can compare the deposition equipment.
| E-beam evaporation (Temescal) | Sputter deposition (Lesker) | Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) | |
|---|---|---|---|
| General description | E-beam deposition of Nb
(line-of-sight deposition) |
Sputter deposition of Nb
(not line-of-sight deposition) |
Sputter deposition of Nb
(not line-of-sight deposition) |
| Pre-clean | Ar ion bombardment | none | RF Ar clean |
| Layer thickness | 10Å to 200 nm* | 10Å to 600 nm** | ask staff, probably similar to old Lesker sputter system |
| Deposition rate | 0.5Å/s to 5Å/s | ~1Å/s | ? Probably similar to old Lesker sputter system |
| Batch size |
|
|
|
| Allowed materials |
|
|
|
| Comment | Substrates get heated during the deposition.
For 100 nm Nb at 2 Å/s, the substrate reached about 105 °C. |
* To deposit layers thicker than 200 nm permission is required to ensure that there is enough metal (contact metal@nanolab.dtu.dk)
** To deposit layers thicker than 600 nm permission is required to ensure that there is enough metal (contact metal@nanolab.dtu.dk)