Specific Process Knowledge/Thin film deposition/Deposition of Nickel: Difference between revisions
| Line 145: | Line 145: | ||
|- | |- | ||
|} | |} | ||
Thickness is measured in 5 points with a stylus profiler. <br> | Thickness is measured in 5 points with a stylus profiler (usually DektakXT). <br> | ||
|} | |} | ||
Revision as of 14:23, 24 June 2025
The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.
Feedback to this page: click here
Nickel deposition
Nickel can be deposited by e-beam evaporation or sputtering at DTU Nanolab. For electroplating you will have to contact other institutes at DTU, e.g., DTU Mechanical Engineering.
Some process information is available here for e-beam evaporated films:
- Stress in e-beam evaporated Ni films: study here (from the now decommissioned Wordentec deposition tool - basic trends in results should be transferable to other e-beam evaporators).
In the chart below you can compare the different deposition equipment:
| E-beam evaporation (E-beam evaporator (Temescal) and E-beam evaporator (10-pockets)) | Sputter deposition (Lesker) | Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) | |
|---|---|---|---|
| General description | E-beam deposition of Nickel | Sputter deposition of Nickel | Sputter deposition of Nickel |
| Pre-clean | Ar ion etch (only in E-beam evaporator Temescal) | RF Ar clean | |
| Layer thickness | 10 Å to 1 µm * | 10 Å to 500 nm ** | 10 Å to 500 nm ** |
| Deposition rate | 1-10 Å/s | Depends on process parameters, about 1 Å/s | Depends on process parameters, at least ~ 4 Å/s, see conditions here |
| Batch size |
|
|
|
| Allowed materials |
|
|
|
| Comment |
|
|
* To deposit a cumulative thickness above 600 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine
** To deposit a cumulative thickness above 200 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine
Quality control of e-beam evaporated Ni films
| Quality control (QC) for the E-beam Evaporator (Temescal) and the E-beam Evaporator (10-pockets) | ||||||||||||||||||
|
Nickel deposition is tested occasionally, around 1 time per year in each machine. Let us know if you notice any problems or would like an extra test of the material. LabManager links require login.
|