Revision as of 11:33, 23 May 2011

nano1.42 versus pxnano2

Recipe nano1.42 pxnano2
Tool Pegasus ASE
Parameters Gas C4F8 75 sccm, SF6 38 sccm
Pressure 4 mTorr, Strike 3 secs @ 15 mTorr
Power 800 W CP, 40 W PP
Temperature -20 degs
Hardware 100 mm Spacers
Time 120 secs
Conditions Run ID 2017
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask 211 nm zep etched down to 82 nm