Jump to content

Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/nano/Sinano4: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
No edit summary
Jmli (talk | contribs)
No edit summary
 
Line 2: Line 2:
<!-- Ok, jmli 20170627 -->
<!-- Ok, jmli 20170627 -->
<!--Checked for updates on 24/8-2021. ok/ jmli-->
<!--Checked for updates on 24/8-2021. ok/ jmli-->
<!--Checked for updates on 4/4-2025 - ok/jmli -->


== The Sinano4.0 recipe ==
== The Sinano4.0 recipe ==

Latest revision as of 08:34, 4 April 2025


The Sinano4.0 recipe

Recipe Sinano4.0
Recipe Gas Cl2 20 sccm
Pressure 2 mTorr, Strike 3 secs @ 5 mTorr
Power 900 W CP, 60 W PP
Temperature 20 degs
Hardware 100 mm Spacers
Time 90 secs
Conditions Run ID 435, ID
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask 110 nm zep etched down to 43 nm
Nominal trench line width ' ' 30 60 90 120 150 Average Std. dev.
Etch rate nm/min 154 169 170 172 177 169 9
Sidewall angle degs 85 83 84 84 84 84 1
CD loss nm/edge 28 52 68 87 101 67 29
CD loss foot nm/edge 28 52 68 87 101 67 29
Bowing 24 28 24 20 16 22 5
Bottom curvature -21 18 20 15 11 9 17
Zep etch rate 45