Jump to content

Specific Process Knowledge/Etch/ICP Metal Etcher/Chromium/End point: Difference between revisions

Bghe (talk | contribs)
Bghe (talk | contribs)
Line 97: Line 97:


|}
|}
=== End point signal===
====Barc etch====
The End point signal shows a top point after 5.5 s and I stopped the etch after 46.4 s giving ''' 41 s after the top point'''.
<gallery caption="S047676 47s barc etch, Feb-2025, wafer center, 100 nm Cr mask, with 500 nm resist" widths="600px" heights="550px" perrow="2">
File:data 03 screen shot 01.jpg
File:data 03 screen shot 02.jpg
</gallery>
====Cr etch====
The End point signal shows a drop after 295 s and I stopped the etch after 465 s giving '''170 s after the drop started'''.
<gallery caption="S047676 7:43 min Cr etch, Feb-2025, wafer center, 100 nm Cr mask, with 500 nm resist" widths="600px" heights="550px" perrow="2">
File:data 05 screen shot 02.jpg
File:data 05 screen shot 04.jpg
</gallery>


==Etched too short==
==Etched too short==