| Line 18: | Line 18: | ||
|- | |- | ||
| | | | ||
<gallery caption="S047676 | <gallery caption="S047676 47s barc etch, 7:43 min Cr etch, Feb-2025, wafer center, 100 nm Cr mask, with 500 nm resist" widths="600px" heights="550px" perrow="1"> | ||
File:S047676midt_cr_14.jpg | File:S047676midt_cr_14.jpg | ||
File:S047676midt_cr_12.jpg | File:S047676midt_cr_12.jpg | ||
Revision as of 17:00, 18 February 2025
Feedback to this page': click here
THIS PAGE IS UNDER CONSTRUCTION
Made by Berit bghe @ DTU Nanolab
Using the standard Cr etch recipe I was etching through 100 nm Cr on a 150 mm wafer it an etch load of 50%
I recorded the end point signal and tried three different stopping times to figure out when to stop the etch. I want to find out how I can use the end point signal to get the best etch result; Etch though - also in the small patterns without too much over etch.
I was looking at trenches with sizes ranging from 200 nm to 2 µm in width. The masking materials was negative DUV resist: NUV 2300-0.5 of approximately 500 nm. Here process flow can be seen here: File:Process_flow_for_test_wafers xx.pdf
Etched close to optimal
| Middel of the wafer | Close to wafer edge |
|---|---|
|
|
Etched too long
| Middel of the wafer | Close to wafer edge |
|---|---|
|
|
Etched too short
| Middel of the wafer | Close to wafer edge |
|---|---|
|
|