AR-N 7520 New is a resist provided by Allresist. The "New" is important, "AR-N 7520" and "AR-N 7520 New" are not the same resists. | |||
=Contrast curve= | =Contrast curve= | ||
* Coater: LabSpin 2 | |||
* Substrate: 2" Si | |||
* Acceleration: 1000 RPM/s | |||
* Speed: 4000 RPM | |||
* Time: 60 s | |||
* Baking temperature: 85C | |||
* Baking time: 90 s | |||
* Exposure: 100 kV (JEOL 9500) | |||
* Development: AR 300-46 for 90 seconds | |||
* Stopper: IPA for 30 seconds + blow dry with nitrogen | |||
Revision as of 10:46, 20 January 2025
AR-N 7520 New is a resist provided by Allresist. The "New" is important, "AR-N 7520" and "AR-N 7520 New" are not the same resists.
Contrast curve
- Coater: LabSpin 2
- Substrate: 2" Si
- Acceleration: 1000 RPM/s
- Speed: 4000 RPM
- Time: 60 s
- Baking temperature: 85C
- Baking time: 90 s
- Exposure: 100 kV (JEOL 9500)
- Development: AR 300-46 for 90 seconds
- Stopper: IPA for 30 seconds + blow dry with nitrogen