Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/SiO2 Etch/Cr mask: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
Bghe (talk | contribs)
Line 84: Line 84:
|}
|}
===Profile SEM images===
===Profile SEM images===
{| border="2" cellspacing="2" cellpadding="3" style="width: 100%;"
{| border="2" cellspacing="2" cellpadding="3" style="width: 100%;"  
!style="width: 20%"|Recipe settings
!style="width: 20%"|Recipe settings
!style="width: 10%"|Comments
!style="width: 10%"|Comments
!style="width: 70%"|SEM gallery
!style="width: 70%"|SEM gallery
|-
|- style="vertical-align:top;"
|
|
*'''On 6" wafer'''
*'''On 6" wafer'''
Line 111: Line 111:
File:C09721_center_22.jpg
File:C09721_center_22.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*'''Piece on Si carrier'''
*'''Piece on Si carrier'''
Line 134: Line 134:
File:C10022_03__12.jpg
File:C10022_03__12.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*Coil Power [W]:2500
*Coil Power [W]:2500
Line 155: Line 155:
File:C10025_03__01.jpg
File:C10025_03__01.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*Coil Power [W]:2500
*Coil Power [W]:2500
Line 177: Line 177:
File:C10026_03__10.jpg
File:C10026_03__10.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*Coil Power [W]:2500
*Coil Power [W]:2500
Line 202: Line 202:
File:C010082tilt30_13.jpg
File:C010082tilt30_13.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*'''Coil Power [W]:1200'''
*'''Coil Power [W]:1200'''
Line 224: Line 224:
File:C10084_03.jpg
File:C10084_03.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*Coil Power [W]:1200
*Coil Power [W]:1200
Line 246: Line 246:
File:C10093_03__01.jpg
File:C10093_03__01.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*Coil Power [W]:1200
*Coil Power [W]:1200
Line 269: Line 269:
File:C10101_03__14.jpg
File:C10101_03__14.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*'''Coil Power [W]:1800'''
*'''Coil Power [W]:1800'''
Line 291: Line 291:
File:C10102_03__16.jpg
File:C10102_03__16.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*Coil Power [W]:1800
*Coil Power [W]:1800
Line 312: Line 312:
File:C10110_12.jpg
File:C10110_12.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*'''Coil Power [W]:1200'''
*'''Coil Power [W]:1200'''
Line 334: Line 334:
File:C10119_11.jpg
File:C10119_11.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*Coil Power [W]:1200
*Coil Power [W]:1200
Line 357: Line 357:
File:Contour Plot Y32 EM_02_30 blue to red.jpg| Etch on none patterned wafer, Uniformity: +- 6.4%
File:Contour Plot Y32 EM_02_30 blue to red.jpg| Etch on none patterned wafer, Uniformity: +- 6.4%
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*'''Coil Power [W]:1800'''
*'''Coil Power [W]:1800'''
Line 381: Line 381:
File:C010161tilt_04.jpg
File:C010161tilt_04.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*'''Coil Power [W]:1200'''
*'''Coil Power [W]:1200'''
Line 409: Line 409:
File:C010184tilt20plasmaO2_05.jpg| tilt 20 degrees
File:C010184tilt20plasmaO2_05.jpg| tilt 20 degrees
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*'''Coil Power [W]:2500'''
*'''Coil Power [W]:2500'''
Line 429: Line 429:
File:C10381_30dg_21.jpg
File:C10381_30dg_21.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*Coil Power [W]:2500
*Coil Power [W]:2500
Line 451: Line 451:
File:C10393_16.jpg
File:C10393_16.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*'''14 min'''
*'''14 min'''
Line 473: Line 473:
File:C10399_13.jpg
File:C10399_13.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*'''Back to start setting without EM coils - 14 min'''
*'''Back to start setting without EM coils - 14 min'''
Line 498: Line 498:
File:C10576_17.jpg
File:C10576_17.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*'''Coil Power [W]:600'''
*'''Coil Power [W]:600'''
Line 519: Line 519:
File:C10751_12.jpg
File:C10751_12.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*'''Coil Power [W]:300'''
*'''Coil Power [W]:300'''
Line 540: Line 540:
File:C10752_10.jpg
File:C10752_10.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*'''45 min'''
*'''45 min'''
Line 568: Line 568:
File:C10834T_22.jpg
File:C10834T_22.jpg
</gallery>
</gallery>
|-
|- style="vertical-align:top;"
|
|
*Coil Power [W]:300
*Coil Power [W]:300

Revision as of 11:32, 8 February 2024

Feedback to this page: click here
Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab

SiO2 trench etching with Cr mask

Start parameters, variations noted in the gallery headline Recipe name: no 10 with lower platen power
Coil Power [W] 2500
Platen Power [W] 200
Platen temperature [oC] 20
H2 flow [sccm] 25.6
C4F8 flow [sccm] 25.6
He flow [sccm] 448.7
Pressure Fully open APC valve (8-9 mTorr)
Electromagnetic coils (EM) 'outer coil' / 'inner coil' '2 A' / '30 A' (PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN)
  • 100 nm Cr mask etched in ICP metal with 500nm DUV neg resist (NUV 2300-0.5) and 65 nm barc.
Cr mask before SiO2 etch 800 nm pitch 50% duty cycle. The The Cr linewidth is clearly less than designed


Results

Temporary conclusions on how the process parameters affect the results in this study: What process parameters affect the results?
  • Going from full wafer to small piece on Si carrier:
    • Seemed to give more sidewall passivation
  • Platen power: lowering the platen power gives
    • more sidewall passivation
    • lower etch rate
    • Less trenching
  • Removing the H2 gave:
    • less sidewall passivation
  • Adding O2 gave:
    • less sidewall passivation
  • Process pressure/total gasflow rate
    • Reducing total gasflow rate which reduced the pressur inside the chamber gave:
      • less sidewall passivation
      • Reduced the CD (Critical Dimensions)
  • Coil power: Reducing coil power
    • less CD loss
    • more sidewall passivation
  • Increasing process time:
    • less sidewall passivation
    • more sidewall bow
    • CD loss due to larger mask faceting
  • Sidewall passivation↑
    • Sample size↓
    • Platen power↓
    • Coil power↓
    • H2 flow↑
    • O2 flow↓
    • Total gas flow rate/pressure↑

Profile SEM images

Recipe settings Comments SEM gallery
  • On 6" wafer
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:25.6
  • C4F8 flow [sccm]: 25.6
  • He flow [sccm]:448.7
  • Pressure:Fully open APC valve (8-9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
text
  • Piece on Si carrier
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:25.6
  • C4F8 flow [sccm]: 25.6
  • He flow [sccm]:448.7
  • Pressure:Fully open APC valve (8-9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
More sidewall passivation on chip than on full wafer
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • C4F8 flow [sccm]: 25.6
  • He flow [sccm]:448.7
  • Pressure:Fully open APC valve (8-9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Less sidewall passivation from removing the H2
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 5
  • C4F8 flow [sccm]: 25.6
  • He flow [sccm]:448.7
  • Pressure:Fully open APC valve (8-9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Not a large effect from adding a little O2
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 0
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:225
  • Pressure:Fully open APC valve (3.35 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Reducing total flow rate and thereby the pressure gives less passivation/redeposition. Sidewall roughness not so bad.
  • Coil Power [W]:1200
  • Platen Power [W]: 150
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 0
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:225
  • Pressure:Fully open APC valve (3.35 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Reducing the coil power a lot and platen power a little gives more sidewall passivation/redeposition
  • Coil Power [W]:1200
  • Platen Power [W]: 150
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 10
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:215
  • Pressure:Fully open APC valve (3.35 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Adding oxygen reduces the passivation/redeposition
  • Coil Power [W]:1200
  • Platen Power [W]: 150
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.35 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Adding more oxygen reduces further the passivation/redeposition but some trenching appears.
  • Coil Power [W]:1800
  • Platen Power [W]: 150
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 10
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:215
  • Pressure:Fully open APC valve (3.35 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Increasing coil power reduces trenching but increases passivation/redeposition
  • Coil Power [W]:1800
  • Platen Power [W]: 150
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.6 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Adding more O2 reduces the sidewall passivation/redeposition
  • Coil Power [W]:1200
  • Platen Power [W]: 100
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.6 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Running with the lower coil power and reducing the platen power also seems to reduced the sidewall passivatin/redeposition, but etch rate goes down
  • Coil Power [W]:1200
  • Platen Power [W]: 100
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.6 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Repeating with longer etch time to etch 1500 nm down. Unfortunately this damaged the hardware due to the EM coils getting too hot.
  • Coil Power [W]:1800
  • Platen Power [W]: 150
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.6 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Running 1800W/150W at increased time to etch down to 1500 nm.
  • Coil Power [W]:1200
  • Platen Power [W]: 100
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
Repeating the 1200W/100W recipes at 14 min but without the EM coils. For this recipe the uniformity over the wafer improved from removing the EM coils, so no need for those and now the recipe could run 14 min without damaging the hardware. The profile looked as before. After removing the Cr I looked from the top and with a tilted view and saw the the sidewall roughness was very bad.
  • Coil Power [W]:2500
  • Platen Power [W]: 100
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
Tried high coil power and low platen power. This seemed to give som undercutting,especially on the narrow lines. The smallest has been etched away. The etch rate was very low
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 0
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:225
  • Pressure:Fully open APC valve (3.9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
Increasing the platen power and and removing the oxygen helped on the under cutting but the lines are still very narrow at the bottom. It also increased the etch rate
  • 14 min
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
Adding the oxygen again further increased the etch rate and reduced the CD (Critical Dimension) of the Cr mask.
  • Back to start setting without EM coils - 14 min
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:25.6
  • O2 flow [sccm]: 0
  • C4F8 flow [sccm]: 25.6
  • He flow [sccm]:448.7
  • Pressure:Fully open APC valve (8-9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
I repeated the start setting but without the EM coils. This gives a very none uniform etch over the wafer where in some parts it deposites instead of etching. The profile of 800 nm oitch look fairly good but a closer look reveals the the sidewall is very rough from either redeposition or polymerization. this cannot be removed with a O2 plasma.
  • Coil Power [W]:600
  • Platen Power [W]: 50
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 10
  • C4F8 flow [sccm]: 6.5
  • He flow [sccm]:100
  • Pressure:Fully open APC valve (<2 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
Due to the large sidewall roughness I decided to try and run at lower powers because it looked at some images like an ionbonbardment effect. First try with 600W/50W. The profile looks fairly good but still with some sidewall roughness. there is also some trenching and the Cr mask looks has a facet all the way down to the SiO2. The is also some bowing.
  • Coil Power [W]:300
  • Platen Power [W]: 25
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 10
  • C4F8 flow [sccm]: 6.5
  • He flow [sccm]:100
  • Pressure:Fully open APC valve (<2 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
Even lower powers: 300W/25W. The profiles looks better with less roughness but also mush slower etch rate, so not as deep as the previous.
  • 45 min
  • Coil Power [W]:300
  • Platen Power [W]: 25
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 10
  • C4F8 flow [sccm]: 6.5
  • He flow [sccm]:100
  • Pressure:Fully open APC valve (<2 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
Repeating with longer etch time. Low sidewall roughness, less faceting of the Cr mask. Still some trenching and bowing or negative tapering of the profile.
  • Coil Power [W]:300
  • Platen Power [W]: 20
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 10
  • C4F8 flow [sccm]: 6.5
  • He flow [sccm]:100
  • Pressure:Fully open APC valve (<2 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
Decreased the platen power a little to see if this could remove the trenching. Not much different from the last.