Line 258: Line 258:
*Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'  
*Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'  
*PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
*PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|Adding more oxygen reduces further the passivation/redeposition
|Adding more oxygen reduces further the passivation/redeposition but some trenching appears.
|
|
<gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1200W" perrow="7" widths="200px" heights="150px">
<gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:205sccm O2:20sccm, Pressure:3.6mTorr; platen power 150W, coil power:1200W" perrow="7" widths="200px" heights="150px">
Line 281: Line 281:
*Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'  
*Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'  
*PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
*PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
|Increasing coil power reduces trenching but increases passivation/redeposition
|
|
|text
<gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W" perrow="6" widths="200px" heights="150px">
<gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:215sccm O2:10sccm, Pressure:3.6mTorr; platen power 150W, coil power:1800W" perrow="6" widths="200px" heights="150px">
File:C10102_03__05.jpg
File:C10102_03__05.jpg

Revision as of 16:11, 6 February 2024

Feedback to this page: click here
Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab

SiO2 trench etching with Cr mask

Start parameters, variations noted in the gallery headline Recipe name: no 10 with lower platen power
Coil Power [W] 2500
Platen Power [W] 200
Platen temperature [oC] 20
H2 flow [sccm] 25.6
C4F8 flow [sccm] 25.6
He flow [sccm] 448.7
Pressure Fully open APC valve (8-9 mTorr)
Electromagnetic coils (EM) 'outer coil' / 'inner coil' '2 A' / '30 A' (PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN)
  • 100 nm Cr mask etched in ICP metal with 500nm DUV neg resist (NUV 2300-0.5) and 65 nm barc.
Cr mask before SiO2 etch 800 nm pitch 50% duty cycle. The The Cr linewidth is clearly less than designed


Results

Temporary conclusions on how the process parameters affect the results in this study: What process parameters affect the results?
  • Going from full wafer to small piece on Si carrier:
    • Seemed to give more sidewall passivation
  • Platen power: lowering the platen power gives
    • more sidewall passivation
    • lower etch rate
    • Less trenching
  • Removing the H2 gave:
    • less sidewall passivation
  • Adding O2 gave:
    • less sidewall passivation
  • Process pressure/total gasflow rate
    • Reducing total gasflow rate which reduced the pressur inside the chamber gave:
      • less sidewall passivation
      • Reduced the CD (Critical Dimensions)
  • Coil power: Reducing coil power
    • less CD loss
    • more sidewall passivation
  • Increasing process time:
    • less sidewall passivation
    • more sidewall bow
    • CD loss due to larger mask faceting
  • Sidewall passivation↑
    • Sample size↓
    • Platen power↓
    • Coil power↓
    • H2 flow↑
    • O2 flow↓
    • Total gas flow rate/pressure↑

Profile SEM images

Recipe settings Comments SEM gallery
  • On 6" wafer
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:25.6
  • C4F8 flow [sccm]: 25.6
  • He flow [sccm]:448.7
  • Pressure:Fully open APC valve (8-9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
text
  • Piece on Si carrier
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:25.6
  • C4F8 flow [sccm]: 25.6
  • He flow [sccm]:448.7
  • Pressure:Fully open APC valve (8-9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
More sidewall passivation on chip than on full wafer
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • C4F8 flow [sccm]: 25.6
  • He flow [sccm]:448.7
  • Pressure:Fully open APC valve (8-9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Less sidewall passivation from removing the H2
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 5
  • C4F8 flow [sccm]: 25.6
  • He flow [sccm]:448.7
  • Pressure:Fully open APC valve (8-9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Not a large effect from adding a little O2
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 0
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:225
  • Pressure:Fully open APC valve (3.35 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Reducing total flow rate and thereby the pressure gives less passivation/redeposition. Sidewall roughness not so bad.
  • Coil Power [W]:1200
  • Platen Power [W]: 150
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 0
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:225
  • Pressure:Fully open APC valve (3.35 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Reducing the coil power a lot and platen power a little gives more sidewall passivation/redeposition
  • Coil Power [W]:1200
  • Platen Power [W]: 150
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 10
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:215
  • Pressure:Fully open APC valve (3.35 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Adding oxygen reduces the passivation/redeposition
  • Coil Power [W]:1200
  • Platen Power [W]: 150
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.35 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Adding more oxygen reduces further the passivation/redeposition but some trenching appears.
  • Coil Power [W]:1800
  • Platen Power [W]: 150
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 10
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:215
  • Pressure:Fully open APC valve (3.35 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
Increasing coil power reduces trenching but increases passivation/redeposition
  • Coil Power [W]:1800
  • Platen Power [W]: 150
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.6 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
text
  • Coil Power [W]:1200
  • Platen Power [W]: 100
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.6 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
text
  • Coil Power [W]:1200
  • Platen Power [W]: 100
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.6 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
text
  • Coil Power [W]:1800
  • Platen Power [W]: 150
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.6 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'2 A' / '30 A'
  • PLEASE DO NOT RUN WITH THESE SETTINGS FOR MORE THAN 6 MIN
text
  • Coil Power [W]:1200
  • Platen Power [W]: 100
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
text
  • Coil Power [W]:2500
  • Platen Power [W]: 100
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
text
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 0
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:225
  • Pressure:Fully open APC valve (3.9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
text
  • 14 min
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 20
  • C4F8 flow [sccm]: 13.0
  • He flow [sccm]:205
  • Pressure:Fully open APC valve (3.9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
text
  • Back to start setting without EM coils - 14 min
  • Coil Power [W]:2500
  • Platen Power [W]: 200
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:25.6
  • O2 flow [sccm]: 0
  • C4F8 flow [sccm]: 25.6
  • He flow [sccm]:448.7
  • Pressure:Fully open APC valve (8-9 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
text
  • Coil Power [W]:600
  • Platen Power [W]: 50
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 10
  • C4F8 flow [sccm]: 6.5
  • He flow [sccm]:100
  • Pressure:Fully open APC valve (<2 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
text
  • Coil Power [W]:300
  • Platen Power [W]: 25
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 10
  • C4F8 flow [sccm]: 6.5
  • He flow [sccm]:100
  • Pressure:Fully open APC valve (<2 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
text
  • 45 min
  • Coil Power [W]:300
  • Platen Power [W]: 25
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 10
  • C4F8 flow [sccm]: 6.5
  • He flow [sccm]:100
  • Pressure:Fully open APC valve (<2 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
text
  • Coil Power [W]:300
  • Platen Power [W]: 20
  • Platen temperature [oC]: 20
  • H2 flow [sccm]:0
  • O2 flow [sccm]: 10
  • C4F8 flow [sccm]: 6.5
  • He flow [sccm]:100
  • Pressure:Fully open APC valve (<2 mTorr)
  • Electromagnetic coils (EM) 'outer coil' / 'inner coil':'0 A' / '0 A'
text