AR-P 617 is a positive PMMA based E-beam resist from Allresist. [https://www.allresist.com/wp-content/uploads/sites/2/2020/03/AR-P610_english_Allresist_product-information.pdf | AR-P 617 is a positive PMMA based E-beam resist from Allresist. [https://www.allresist.com/wp-content/uploads/sites/2/2020/03/AR-P610_english_Allresist_product-information.pdf Process information provided by Allresist can be found here.] | ||
=Spin coating= | =Spin coating= | ||
Revision as of 12:56, 22 January 2024
AR-P 617 is a positive PMMA based E-beam resist from Allresist. Process information provided by Allresist can be found here.
Spin coating
AR-P 617 can be spin coated on LabSpin 2 and 3 using the CSAR/PMMA bowlset. A spin curve for AR-P 617.06 is provided below. Process parameters are:
- Date: January 22nd 2024
- Coater: LabSpin 3
- Substrate: 2" Si
- Acceleration: 1000 RPM/s
- Time: 60 s
- Baking temperature: 200C (setpoint at 222C)
- Baking time: 120 s
|
AR-P 617.06 spin curve. |