*Almost that does not degas also if you plan to heat the substrate - see cross contamination sheets for [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 PC1] and [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 PC3] |-style="background:WhiteSmoke; color:black" | *Almost that does not degas also if you plan to heat the substrate - see cross contamination sheets for [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 PC1] and [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 PC3] |-style="background:WhiteSmoke; color:black" | ||
|} | |} | ||
Revision as of 15:52, 19 January 2024
Feedback to this page: click here
Unless otherwise stated, this page is written by DTU Nanolab internal
Deposition of Cu
Copper can be deposited by e-beam evaporation or sputtering at Nanolab. In the chart below you can compare the different deposition equipment. Further down you will find some results of studies on Cu deposition processes.
| E-beam evaporation (E-beam evaporator (Temescal) and E-beam evaporator (10-pockets)) | Sputter deposition (Lesker) | Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) | |
|---|---|---|---|
| General description | E-beam deposition of Cu
(line-of-sight deposition) |
Sputter deposition of Cu
(not line-of-sight deposition) |
Sputter deposition of Cu
(not line-of-sight deposition) |
| Pre-clean | Ar ion etch (only in E-beam evaporator Temescal) | RF Ar clean | RF Ar clean |
| Layer thickness | 10Å to 1µm* | 10Å to 1µm** | 10Å to 1µm** |
| Deposition rate | 1-10 Å/s | ~ 1 Å/s | Depends on process parameters, at least up to 8.7 Å/s, see conditions here |
| Batch size |
|
|
|
| Allowed materials |
|
|
* To deposit layers thicker than 600 nm permission is required to ensure that there is enough metal (contact metal@nanolab.dtu.dk)
** To deposit layers thicker than 200 nm permission is required to ensure that there is enough metal (contact metal@nanolab.dtu.dk)
Studies of Cu deposition
Roughness of Cu layers - Roughness of Cu layers deposited with the Alcatel e-beam evaporator
Stress in sputtered Cu - Low stress in Cu films sputtered with the Sputter-System (Lesker)