Specific Process Knowledge/Thermal Process/RTP Jipelec 2: Difference between revisions
| Line 88: | Line 88: | ||
|style="background:Silver; color:black"|At 1200 <sup>o</sup>C | |style="background:Silver; color:black"|At 1200 <sup>o</sup>C | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
*Max. | *Max. 1 minute | ||
|style="background:WhiteSmoke; color:black;" align="center"| | |style="background:WhiteSmoke; color:black;" align="center"| | ||
|- | |- | ||
|style="background:Silver; color:black"|At 1100 <sup>o</sup>C | |style="background:Silver; color:black"|At 1100 <sup>o</sup>C | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
*Max. | *Max. 5 minutes | ||
|style="background:WhiteSmoke; color:black;" align="left"| | |style="background:WhiteSmoke; color:black;" align="left"| | ||
|- | |- | ||
|style="background:Silver; color:black"|At 1000 <sup>o</sup>C | |style="background:Silver; color:black"|At 1000 <sup>o</sup>C | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
*Max. | *Max. 10 minutes | ||
|style="background:WhiteSmoke; color:black;" align="left"| | |||
|- | |||
|style="background:Silver; color:black"|At 900 <sup>o</sup>C | |||
|style="background:LightGrey; color:black"| | |||
*Max. 20 minutes | |||
|style="background:WhiteSmoke; color:black;" align="left"| | |||
|- | |||
|style="background:Silver; color:black"|At 800 <sup>o</sup>C | |||
|style="background:LightGrey; color:black"| | |||
*Max. 30 minutes | |||
|style="background:WhiteSmoke; color:black;" align="left"| | |||
|- | |||
|style="background:Silver; color:black"|At 700 <sup>o</sup>C | |||
|style="background:LightGrey; color:black"| | |||
*Max. 1 hour | |||
|style="background:WhiteSmoke; color:black;" align="left"| | |||
|- | |||
|style="background:Silver; color:black"|< 700 <sup>o</sup>C | |||
|style="background:LightGrey; color:black"| | |||
*Max. 2 hours | |||
|style="background:WhiteSmoke; color:black;" align="left"| | |||
|- | |||
|style="background:Silver; color:black"|< 500 <sup>o</sup>C | |||
|style="background:LightGrey; color:black"| | |||
*Max. 5 hours | |||
|style="background:WhiteSmoke; color:black;" align="left"| | |style="background:WhiteSmoke; color:black;" align="left"| | ||
|- | |- | ||
Revision as of 16:17, 6 November 2023
Feedback to this page: click here
This page is written by DTU Nanolab internal
THIS PAGE IS UNDER CONSTRUCTION
RTP2 Jipelec - Rapid Thermal Processor

The main purpose of the RTP2 Jipelec (Jipelec JetFirst 200 RTP) is to perform thermal processes, using faster heating rates and shorter process durations when compared to conventional methods. This is called rapid thermal processing (RTP) and can be used to treat different types of samples.
Rapid thermal processing typically includes RTA, i.e. Rapid Thermal Annealing, where samples are heated up very rapidly in a nitrogen or argon atmosphere. Contact alloying and RTN, i.e. Rapid Thermal Nitridation, might also be possible for some samples.
The Set-Up
The machine consists of a reactor chamber, in which different samples can be processed/annealed at temperatures up to 1200 °C.
The chamber can be heated up very rapidly by the use of 18 infrared halogen lamps that are situated in the chamber lid. A quartz plate is placed below the lamps, i.e. between the lamps and the sample(s). Below the platen, there is an optical pyrometer aligned with the center of the substrate, that is placed on the bottom part of the chamber. The platen presents additional inlets where multiple thermocouples can be mounted. These details are exemplified in the images on the right.
[[|400px|thumb|Schematic representation of the RTP2 Jipelec reactor. Image: DTU Nanolab]]

The lamps are divided in three zones so that a uniform temperature can be obtained over the substrate. During the heating, the quartz window below the lamps will get warm. However, the chamber walls are cooled by a cooling water flow and thus remain cold to prevent sample contamination. As already mentioned, the cooling unit is located under the machine. The lamps are cooled by cooling fans (no noisy compressed air cooling like in the old Jipelec RTP). The halogen lamps and the quartz plate are visible in the image below.

The samples are placed above the round metal plate in the bottom of the chamber, i.e. below the halogen lamps. The substrates are meant to be placed on top of three quartz pins. Depending on the type and size of the substrate, there are three types of quartz pins available (for the SiC-coated graphite susceptor, a 100 mm wafer and for a 150 mm wafer). Nonetheless, the susceptor should always be used, when possible (except for 8" wafers).

Temperature Measurement and Control
Samples and Process Specifications
| Specifics | Range | Comments | |
|---|---|---|---|
| Temperature | Pyro Control |
|
|
| Thermocouple Control |
|
||
| Process gas | Argon (Ar) |
|
|
| Nitrogen (N2) |
|
||
| Forming gas (4% H2/ 96% N2) |
|
Gas line not connected yet. | |
| Nitrogen purge (N2) |
|
Do not use for processing. | |
| Pressure | No vacuum |
|
|
| Vacuum |
|
5/6 mbar, if minimum gas flow is used during process. | |
| Process time
(Check image below) |
At 1200 oC |
|
|
| At 1100 oC |
|
||
| At 1000 oC |
|
||
| At 900 oC |
|
||
| At 800 oC |
|
||
| At 700 oC |
|
||
| < 700 oC |
|
||
| < 500 oC |
|
||
| Heating rate |
|
At faster heating rates, the actual temperature might overshoot from the temperature setpoint in the recipe, and the susceptors/carriers might break. | |
| Substrates | Batch size |
|
|
| Substrate size |
|
Small samples must be placed on dedicated carrier wafers/susceptors. These do not need to and should not be bonded to the carriers. | |
| Allowed materials |
|
Always check the cross contamination information in LabManager to see whether your samples are allowed in the RTP2 Jipelec before using it. If you want to anneal sample materials that are not on the list or not approved, please contact the Thin Film group | |
Remark! The time limits are not implemented in the software, but it is very important to obey these. If processing is done for longer times than those defined in the table, there is a certain risk that the chamber gets overheated, which can lead to damage of the equipment.
Additional information
The user manual, user APV, technical and contact information can be found in LabManager: RTP2 Jipelec