Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/SiO2 Etch/Cr mask: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
No edit summary
Bghe (talk | contribs)
No edit summary
Line 92: Line 92:
<gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr; platen power 150W, coil power:1200W" perrow="6" widths="200px" heights="150px">
<gallery caption="SiO2 etch with Cr mask on wafer piece on Si carrier 6 min etch, H2:0sccm, C4F8:13sccm He:225sccm, Pressure:3.35mTorr; platen power 150W, coil power:1200W" perrow="6" widths="200px" heights="150px">
File:C10084_15.jpg
File:C10084_15.jpg
File:C10084_13.jpg
File:C10084_11.jpg
File:C10084_09.jpg
File:C10084_06.jpg
File:C10084_03.jpg
File:C10084_03.jpg
File:C10084_06.jpg
 
File:C10084_09.jpg
File:C10084_11.jpg
File:C10084_13.jpg
</gallery>
</gallery>

Revision as of 10:56, 26 September 2023

Feedback to this page: click here
Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab

Start parameters, variations noted in the gallery headline Recipe name: no 10 with lower platen power
Coil Power [W] 2500
Platen Power [W] 200
Platen temperature [oC] 20
H2 flow [sccm] 25.6
C4F8 flow [sccm] 25.6
He flow [sccm] 448.7
Pressure Fully open APC valve (8-9 mTorr)
Electromagnetic coils (EM) 'outer coil' / 'inner coil' '2 A' / '30 A'
  • 100 nm Cr mask etched in ICP metal with 500nm DUV neg resist and 65 nm barc.