Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4/Slow etch: Difference between revisions
Appearance
| Line 62: | Line 62: | ||
<br clear="all" /> | <br clear="all" /> | ||
<gallery> | <gallery caption="Map of etch rate measurements" widths="250px" heights="250px" perrow="2"> | ||
File:contour plot for etchrate of slow etch in SiO2.JPG | File:contour plot for etchrate of slow etch in SiO2.JPG| Etch rate map of SiO2 etch on 6" wafer | ||
File:contour plot for etchrate of slow etch in SRN.JPG | File:contour plot for etchrate of slow etch in SRN.JPG| Etch rate map of SRN etch on 6" wafer | ||
</gallery> | </gallery> | ||
Revision as of 16:53, 6 December 2022
The slow etch
The slow etch is designed to etch slow at low powers to etch thin films and to avoid overheating of samples mounted on a carrier with Capton/polyimide tape
| Parameter | Recipe name: Slow Etch |
|---|---|
| Coil Power [W] | 350 |
| Platen Power [W] | 25 |
| Platen temperature [oC] | 20 |
| He flow [sccm] | 0 |
| CF4 flow [sccm] | 45 |
| Pressure [mTorr] | 3 |
| Typical results | Test Results |
|---|---|
| Etch of SRN | ~43nm/min [measured 39-50 nm/min over a 6" wafer] |
| Etch rate of Si3N4 | ~49nm/min [4" on carrier] |
| Etch rate of SiO2 | ~42nm/min [41-43 nm/min over a 6" wafer] |
| Etch rate of DUV resist] | ~nm/min
|
| Profile [o] |
- Map of etch rate measurements
-
Etch rate map of SiO2 etch on 6" wafer
-
Etch rate map of SRN etch on 6" wafer