Jump to content

Specific Process Knowledge/Wafer and sample drying/Critical Point Dryer: Difference between revisions

From LabAdviser
Kn (talk | contribs)
No edit summary
Kn (talk | contribs)
No edit summary
Line 56: Line 56:




After drying wafers in air, the majority of the cantilevers are bended and sticking to the underlying surface.
After drying wafers in air, the majority of the cantilevers are bended and sticking to the underlying surface. But after the wafers were dried in Critical point dryer, the cantilevers were free hanging.
 


'''Dried in air'''
[[Image:SiN dried air.jpg|350x350px|left|thumb|Dried in air: most cantilevers are bended.]]
[[Image:SiN dried air.jpg|350x350px|left|thumb|Dried in air: most cantilevers are bended.]]
Dried in air: most cantilevers are bended.
Dried in air: most cantilevers are bended.


'''Dried in CPD'''
[[Image:SiN cantilever dried CPD.jpg|350x350px|left|thumb|Dried with Critical Point Dryer. ]]
[[Image:SiN cantilever dried CPD.jpg|350x350px|left|thumb|Dried with Critical Point Dryer. ]]


Line 67: Line 69:
Dried with Critical Point Dryer. The cantilevers are free hanging, and have not bended. The dimensions of the cantilevers are 100 x 710 µm, and the thickness is about 0.5 µm.
Dried with Critical Point Dryer. The cantilevers are free hanging, and have not bended. The dimensions of the cantilevers are 100 x 710 µm, and the thickness is about 0.5 µm.


Pic 3
[[Image:SiN cantilever dried CPD nr7.jpg|350x350px|left|thumb|Dried with Critical Point Dryer.]]
 
Dried with the Critical Point Dryer. The cantilevers structures are free hanging after the drying.
Dried with the Critical Point Dryer. The cantilevers structures are free hanging after the drying.



Revision as of 17:30, 17 February 2010

Critical Point Dryer

Critical point dryer: positioned in cleanroom 4

The critical point dryer is used to dry fragile structures that may be damaged in a normal drying procedure. Fragile structures may be thin membranes, or free hanging structures like cantilevers and grippers.

In the critical point dryer, these structures are dried in CO2. In the drying process, the sample is first put into Isopropanol, and loaded into the machine. In the process itself, the isopropanol is exchanged for liquid CO2. When there is only CO2 in the machine, the pressure and temperature in the chamber is raised, above the so called “critical point”. In this way, there is never a liquid/gas interface, but instead the liquid is turned into a mixture of equal parts of gas and liquid. Because of this, the problem with surface tension, which destroys the fragile structures through capillary forces, is avoided.


Purpose Drying of wafers or chips

To dry fragile structures (example membranes, grippers, cantilevers).

Process parameter range Process Temperature

0oC temperature to 45oC

Process pressure

1 atm to (maximum) 95 atm (1400 PSI)

Substrates Batch size
  • 1 to 5 wafers per run. Sizes: 2”, 4" or 6" or
  • Pieces (up to 10x10mm)
Substrate material allowed
  • Silicon wafers
  • Quartz wafers
  • Pyrex wafers
  • InAlP
  • GaAs
Material allowed on the substrate
  • Silicon oxide
  • Silicon nitride
  • Poly Silicon
  • SU-8


Comparison of samples dried in air and with Critical Point Dryer

This shows a comparison of samples that have been dried in the critical point dryer, and samples that have been dried in air. Below are pictures of two wafers that have been prepared in the same way- but dried with different methods after the final etching step. Cantilevers of SiN, up to 710 µm long and 100 µm wide, are fabricated in the etching step. The thickness of the cantilevers is about 0.5 µm


After drying wafers in air, the majority of the cantilevers are bended and sticking to the underlying surface. But after the wafers were dried in Critical point dryer, the cantilevers were free hanging.

Dried in air

Dried in air: most cantilevers are bended.

Dried in air: most cantilevers are bended.


Dried in CPD

Dried with Critical Point Dryer.


Dried with Critical Point Dryer. The cantilevers are free hanging, and have not bended. The dimensions of the cantilevers are 100 x 710 µm, and the thickness is about 0.5 µm.

Dried with Critical Point Dryer.

Dried with the Critical Point Dryer. The cantilevers structures are free hanging after the drying.


An acknowledgment goes to Tom Larsen, Nanoprobes, DTU Nanotech, who provided the pictures.