PECVD nitride can be deposited in one of the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] systems. You can run 1-3 wafers at a time depending on which one of the PECVD's you use. The deposition takes place at 300 degrees Celcius. This can be  off importance for some applications but it gives a less dense film and the stoichiometry is on the following form: Si<sub>x</sub>N<sub>y</sub>H<sub>z</sub>. The step coverage and thickness uniformity of the film is not as good as for the LPCVD nitride. In one of our PECVD systems (PECVD3) we allow small amounts of metal on the wafers entering the system, this is not allowed in the LPCVD and in the other PECVD (PECVD1).
PECVD nitride can be deposited in one of the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] systems. You can run 1-3 wafers at a time depending on which one of the PECVD's you use. The deposition takes place at 300 degrees Celcius. This can be  off importance for some applications but it gives a less dense film and the stoichiometry is on the following form: Si<sub>x</sub>N<sub>y</sub>H<sub>z</sub>. The step coverage and thickness uniformity of the film is not as good as for the LPCVD nitride. In one of our PECVD systems (PECVD3) we allow small amounts of metal on the wafers entering the system, this is not allowed in the LPCVD and in the other PECVD (PECVD1).


==comparison of LPCVD and PECVD for silicon nitride deposition==
==Comparison of LPCVD and PECVD for silicon nitride deposition==
{| border="1" cellspacing="0" cellpadding="3" align="center"
{| border="1" cellspacing="0" cellpadding="3" align="center"
!  
!  
Line 30: Line 30:
*~40nm - 10µm
*~40nm - 10µm
|-
|-
|Process Temperature
|
*800-835 <sup>o</sup>C
|
*300 <sup>o</sup>C
|-
|Step coverage
|
*Good
|
*Less good
|-
|Film quality
|
*Dense film
*Few defects
|
*Less dense film
*Incorporation of hydrogen in the film
|-
|Process volume
|
*1-15 4" wafer per run
*deposition on both sides of the substrate
|
*1-3 4" wafers or 1 6" wafer or many smaller chips per run
*deposition on one side of the substrate
|-
| Substrate material allowed
|
*Silicon wafers
**with layers of silicon oxide or silicon (oxy)nitride
*Quartz wafers
|
*Silicon
*Quartz
*Small amount of metal (in PECVD3)
|-
|}
|}



Revision as of 13:17, 24 October 2007

Deposition of Silicon Nitride can be done with either LPCVD, PECVD or sputter deposition.

Deposition of Silicon Nitride using LPCVD

LPCVD nitride can be made in the LPCVD nitride furnace. It is a batch process meaning you can run a batch of 25 wafers at a time. The deposition takes place at temperatures of 800-850 degrees Celcius. The LPCVD nitride has a good step coverage and the film thickness is very uniform over the wafer. We have two standard LPCVD nitride processes: One for depositing stoichiometric nitride (Si3N4) and one for deposition low stress nitride (SNR).

Deposition of Silicon Nitride using PECVD

PECVD nitride can be deposited in one of the PECVD systems. You can run 1-3 wafers at a time depending on which one of the PECVD's you use. The deposition takes place at 300 degrees Celcius. This can be off importance for some applications but it gives a less dense film and the stoichiometry is on the following form: SixNyHz. The step coverage and thickness uniformity of the film is not as good as for the LPCVD nitride. In one of our PECVD systems (PECVD3) we allow small amounts of metal on the wafers entering the system, this is not allowed in the LPCVD and in the other PECVD (PECVD1).

Comparison of LPCVD and PECVD for silicon nitride deposition

LPCVD PECVD
Stoichiometry
  • Si3N4
  • SRN

SRN: Silicon rich nitride

  • SixNyHz
  • SixOyNzHv

Can be doped with boron, phosphorus or germanium

Film thickness
  • Si3N4:~50Å - ~3000Å
  • SRN: ~50Å - ~10000Å
  • ~40nm - 10µm
Process Temperature
  • 800-835 oC
  • 300 oC
Step coverage
  • Good
  • Less good
Film quality
  • Dense film
  • Few defects
  • Less dense film
  • Incorporation of hydrogen in the film
Process volume
  • 1-15 4" wafer per run
  • deposition on both sides of the substrate
  • 1-3 4" wafers or 1 6" wafer or many smaller chips per run
  • deposition on one side of the substrate
Substrate material allowed
  • Silicon wafers
    • with layers of silicon oxide or silicon (oxy)nitride
  • Quartz wafers
  • Silicon
  • Quartz
  • Small amount of metal (in PECVD3)

Choose deposition technique