Etch rate are depending on the level of oxidation of the metal.
Etch rate are depending on the level of oxidation of the metal.


<br clear="all" />


===Overview of the data for the chromium etches===
===Overview of the data for the chromium etches===

Revision as of 15:53, 9 November 2009

Etching of Chromium

Fume hood: positioned in cleanroom 2.
Wet Etch of Chromium can take place in a beaker in this fume hood

Etching of chromium is done wet at Danchip making your own set up in a beaker in a fume hood - preferably in cleanroom 2 or 4. We have two solution for this:

  1. HNO3:H2O:cerisulphate - 90ml:1200ml:15g - standard at Danchip
  2. Commercial chromium etch

Etch rate are depending on the level of oxidation of the metal.



Overview of the data for the chromium etches

Chromium etch 1 Chromium etch 2
General description

Etch of chromium

Etch of chromium

Chemical solution HNO3:H2O:cerisulphate - 90ml:1200ml:15g .
Process temperature Room temperature .
Possible masking materials

Photoresist (1.5 µm AZ5214E)

.

Etch rate

~40-100 nm/min

.

Batch size

1-25 wafers at a time

.

Size of substrate

4" wafers

.

Allowed materials

No restrictions. Make a note on the bottle of which materials have been processed.

.