Specific Process Knowledge/Etch/Etching of Chromium: Difference between revisions
Appearance
| Line 23: | Line 23: | ||
| '''Chemical solution''' | | '''Chemical solution''' | ||
|HNO<math>_3</math>:H<math>_2</math>O:cerisulphate - 90ml:1200ml:15g | |HNO<math>_3</math>:H<math>_2</math>O:cerisulphate - 90ml:1200ml:15g | ||
| | |. | ||
|- | |- | ||
| '''Process temperature''' | | '''Process temperature''' | ||
|Room temperature | |Room temperature | ||
| | |. | ||
|- | |- | ||
| Line 37: | Line 36: | ||
Photoresist (1.5 µm AZ5214E) | Photoresist (1.5 µm AZ5214E) | ||
| | | | ||
. | |||
|- | |- | ||
|'''Etch rate''' | |'''Etch rate''' | ||
| Line 43: | Line 42: | ||
~40-100 nm/min | ~40-100 nm/min | ||
| | | | ||
. | |||
|- | |- | ||
|'''Batch size''' | |'''Batch size''' | ||
| Line 49: | Line 48: | ||
1-25 wafers at a time | 1-25 wafers at a time | ||
| | | | ||
. | |||
|- | |- | ||
|'''Size of substrate''' | |'''Size of substrate''' | ||
| Line 55: | Line 54: | ||
4" wafers | 4" wafers | ||
| | | | ||
. | |||
|- | |- | ||
|'''Allowed materials''' | |'''Allowed materials''' | ||
| Line 62: | Line 61: | ||
Make a note on the bottle of which materials have been processed. | Make a note on the bottle of which materials have been processed. | ||
| | | | ||
. | |||
|- | |- | ||
|} | |} | ||
Revision as of 15:50, 9 November 2009
Etching of Chromium

Wet Etch of Chromium can take place in a beaker in this fume hood
Etching of chromium is done wet at Danchip making your own set up in a beaker in a fume hood - preferably in cleanroom 2 or 4. We have two solution for this:
- HNO:HO:cerisulphate - 90ml:1200ml:15g - standard at Danchip
- Commercial chromium etch
Etch rate are depending on the level of oxidation of the metal.
Overview of the data for the chromium etches
| Chromium etch 1 | Chromium etch 2 | |
|---|---|---|
| General description |
Etch of chromium |
Etch of chromium |
| Chemical solution | HNO:HO:cerisulphate - 90ml:1200ml:15g | . |
| Process temperature | Room temperature | . |
| Possible masking materials |
Photoresist (1.5 µm AZ5214E) |
. |
| Etch rate |
~40-100 nm/min |
. |
| Batch size |
1-25 wafers at a time |
. |
| Size of substrate |
4" wafers |
. |
| Allowed materials |
No restrictions. Make a note on the bottle of which materials have been processed. |
. |