Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/Deposition of Silicon Oxide using Lesker sputter tool: Difference between revisions
| Line 3: | Line 3: | ||
=Sputter deposition of SiO<sub>2</sub> using Sputter System (Lesker)= | =Sputter deposition of SiO<sub>2</sub> using Sputter System (Lesker)= | ||
SiO<sub>2</sub> can be sputter deposited with RF bias in the [[Specific_Process_Knowledge/Thin_film_deposition/Lesker| | SiO<sub>2</sub> can be sputter deposited with RF bias in the Sputter System (Lesker). You can find basic information about the pressure and max power to use and the expected deposition rate on the [[Specific_Process_Knowledge/Thin_film_deposition/Lesker|Equipment page]] here in LabAdviser. To see the deposition parameters used by others, look in the [http://labmanager.dtu.dk/function.php?module=Processlog&view=editlog&machid=244 Process Log] in LabManager. Below you will find deposition parameters and results of a study on the surface roughness and oxide insulation quality of the deposited films. | ||
==Surface roughness optimization== | ==Surface roughness optimization== | ||
| Line 32: | Line 32: | ||
<br> | <br> | ||
==Oxide insulation analysis== | |||
''by Bjarke Thomas Dalslet @Nanotech.dtu.dk'' | |||
The wafers in this analysis consisted of a Si substrate with no native oxide. A layer of SiO<math>_2</math> was reactively sputtered (9% O2 90 W 3.5 mTorr). After that, using a shadow mask, 200nm thick gold rectangles was electro deposited on top of the oxide. Gold was also electro deposited on the back side. Then the impedance as a function of frequency was recorded. | |||
The figure shows the measurements for different oxide thicknesses. Most of the measurements show perfect capacitors, although for illustration measurements with a few pinholes and with many pinholes is also shown for the 20 nm sample. | |||
The success rate for the different thicknesses can be seen in the table, together with the number of samples measured and the number of perfect capacitors. | |||
It is possible to make perfect capacitors with oxide thicknesses down to and including 5 nm and possibly even thinner, although the failure rate increases. Bear in mind, though that each structure measured here has an area of 8 mm<sup>2</sup> - for a 1 mm<sup>2</sup> structure the failure rate would be much lower, assuming the short circuits are not located on the sides of the structures. | |||
[[Image:Lesker_Impedance_Bjarke.png|600px|alt text]] | |||
{| {{table}} border="1" cellspacing="0" cellpadding="8" | |||
| align="center" style="background:#f0f0f0;"|'''Name''' | |||
| align="center" style="background:#f0f0f0;"|'''Thickness [nm]''' | |||
| align="center" style="background:#f0f0f0;"|'''# samples measured''' | |||
| align="center" style="background:#f0f0f0;"|'''# good capacitors''' | |||
| align="center" style="background:#f0f0f0;"|'''Success rate [%]''' | |||
|- | |||
| 38||5||11||1||9 | |||
|- | |||
| 39||10||10||2||20 | |||
|- | |||
| 40||20||7||3||43 | |||
|- | |||
| 41||30||7||7||100 | |||
|- | |||
| 37||50||7||7||100 | |||
|- | |||
|} | |||
<br> | <br> | ||
==Tensile stress in SiO<sub>2</sub> films deposited at high temperature== | ==Tensile stress in SiO<sub>2</sub> films deposited at high temperature== | ||
In 2017 Radu Malureanu deposited SiO<sub>2</sub> at 600 °C in order to obtain films with a high tensile stress. More information on this study can be found [[Specific_Process_Knowledge/Thin_film_deposition/Lesker/Stress_dependence_on_sputter_parameters_in_the_Lesker_sputter_system|here]]. | In 2017 Radu Malureanu deposited SiO<sub>2</sub> at 600 °C in order to obtain films with a high tensile stress. More information on this study can be found [[Specific_Process_Knowledge/Thin_film_deposition/Lesker/Stress_dependence_on_sputter_parameters_in_the_Lesker_sputter_system|here]]. | ||
Revision as of 15:42, 24 March 2020
Feedback to this page: click here
Sputter deposition of SiO2 using Sputter System (Lesker)
SiO2 can be sputter deposited with RF bias in the Sputter System (Lesker). You can find basic information about the pressure and max power to use and the expected deposition rate on the Equipment page here in LabAdviser. To see the deposition parameters used by others, look in the Process Log in LabManager. Below you will find deposition parameters and results of a study on the surface roughness and oxide insulation quality of the deposited films.
Surface roughness optimization
By Bjarke Thomas Dalslet @Nanotech.dtu.dk
The Lesker CMS 18 sputter system provides thin films of varying surface roughness. This roughness was verified to be dependent on the sputtered material, sputter mode (DC or RF) and the substrate bias strength. Other probable factors include sputter power and pressure. Below is a table of results for SiO2. Similar studies were carried out for Si and Ta.
The "From SiO target (RF sputter)" study was done on clean Si substrates. The sputter power was 157W and the pressure 3.5 mTorr using RF sputtering of a SiO target. The film thicknesses were around 42 nm.
From SiO2 target (RF sputter)
| Wafer nr | RF bias (W) | Reactive O2 (%) | Power(W) | Rq (RMS) (nm) | Thickness |
| 3 | 0 | 0 | 157 | 0.902 | |
| 6 | 5 | 0 | 157 | 0.499 | 44 |
| 7 | 10 | 0 | 157 | 0.142 | 42 |
| 8 | 15 | 0 | 157 | 0.422 | 40 |
Oxide insulation analysis
by Bjarke Thomas Dalslet @Nanotech.dtu.dk
The wafers in this analysis consisted of a Si substrate with no native oxide. A layer of SiO was reactively sputtered (9% O2 90 W 3.5 mTorr). After that, using a shadow mask, 200nm thick gold rectangles was electro deposited on top of the oxide. Gold was also electro deposited on the back side. Then the impedance as a function of frequency was recorded.
The figure shows the measurements for different oxide thicknesses. Most of the measurements show perfect capacitors, although for illustration measurements with a few pinholes and with many pinholes is also shown for the 20 nm sample.
The success rate for the different thicknesses can be seen in the table, together with the number of samples measured and the number of perfect capacitors.
It is possible to make perfect capacitors with oxide thicknesses down to and including 5 nm and possibly even thinner, although the failure rate increases. Bear in mind, though that each structure measured here has an area of 8 mm2 - for a 1 mm2 structure the failure rate would be much lower, assuming the short circuits are not located on the sides of the structures.
| Name | Thickness [nm] | # samples measured | # good capacitors | Success rate [%] |
| 38 | 5 | 11 | 1 | 9 |
| 39 | 10 | 10 | 2 | 20 |
| 40 | 20 | 7 | 3 | 43 |
| 41 | 30 | 7 | 7 | 100 |
| 37 | 50 | 7 | 7 | 100 |
Tensile stress in SiO2 films deposited at high temperature
In 2017 Radu Malureanu deposited SiO2 at 600 °C in order to obtain films with a high tensile stress. More information on this study can be found here.