image:Kaempe_Lesker_standard_recipe_name.png| Deposition rate of HfO<sub>2</sub> at 150 <sup>o</sup>C. Substrate: Silicon 6" wafer with native oxide.
image:Kaempe_Lesker_standard_recipe_name.png| Deposition rate of HfO<sub>2</sub> at 150 <sup>o</sup>C. Substrate: Silicon 6" wafer with native oxide.
</gallery>
</gallery>
{| border="2" cellspacing="0" cellpadding="9"
!colspan="1" border="none" style="background:silver; color:black;" align="center"|Recipe name
|style="background:silver; color:black"|<b>Target material</b>
|style="background:silver; color:black"|<b>Pressure (mTorr)</b>
|style="background:silver; color:black"|<b>Power (W)</b>
|style="background:silver; color:black"|<b>Deposition rate (nm/min)</b>
|style="background:silver; color:black"|<b>Uniformity (%)<br> on 6 inch wafer</b>
|style="background:silver; color:black"|<b>Comments</b>
|-
!style="background:silver; color:black;" align="center" |MD PC1 Src1 RF Upstream
|style="background:LightGrey; color:black" align="center"|<b>SiO<sub>2</sub></b>
|style="background:WhiteSmoke; color:black" align="center"|3
|style="background:WhiteSmoke; color:black" align="center"|140 (RF)
|style="background:WhiteSmoke; color:black" align="center"|2.3
|style="background:WhiteSmoke; color:black" align="center"|0.5
|style="background:WhiteSmoke; color:black" align="center"|
|-
!style="background:silver; color:black;" align="center" |MD PC1 Src2 RF Upstream
|style="background:LightGrey; color:black" align="center"|<b>SiO<sub>2</sub></b>
|style="background:WhiteSmoke; color:black" align="center"|3
|style="background:WhiteSmoke; color:black" align="center"|140 (RF)
|style="background:WhiteSmoke; color:black" align="center"|2.6
|style="background:WhiteSmoke; color:black" align="center"|3
|style="background:WhiteSmoke; color:black" align="center"|
|-
!style="background:silver; color:black;" align="center" |MD PC1 Src3 DC Upstream
|style="background:LightGrey; color:black" align="center"|<b>Ni</b>
|style="background:WhiteSmoke; color:black" align="center"|3
|style="background:WhiteSmoke; color:black" align="center"|500 (DC)
|style="background:WhiteSmoke; color:black" align="center"|23.3
|style="background:WhiteSmoke; color:black" align="center"|2.5
|style="background:WhiteSmoke; color:black" align="center"|
|-
!style="background:silver; color:black;" align="center" |MD PC1 Src4 DC Upstream
|style="background:LightGrey; color:black" align="center"|<b>Cu</b>
|style="background:WhiteSmoke; color:black" align="center"|3
|style="background:WhiteSmoke; color:black" align="center"|500 (DC)
|style="background:WhiteSmoke; color:black" align="center"|52.2
|style="background:WhiteSmoke; color:black" align="center"|2.2
|style="background:WhiteSmoke; color:black" align="center"|
|-
!style="background:silver; color:black;" align="center" |MD PC1 Src5 DC Upstream
|style="background:LightGrey; color:black" align="center"|<b>Al</b>
|style="background:WhiteSmoke; color:black" align="center"|3
|style="background:WhiteSmoke; color:black" align="center"|200 (DC)
|style="background:WhiteSmoke; color:black" align="center"|7.9
|style="background:WhiteSmoke; color:black" align="center"|3.2
|style="background:WhiteSmoke; color:black" align="center"|
|-
!style="background:silver; color:black;" align="center" |MD PC1 Src5 Pulse DC<br> Downstream with reactive O<sub>2</sub>
|style="background:LightGrey; color:black" align="center"|<b>Cu</b>
|style="background:WhiteSmoke; color:black" align="center"|3
|style="background:WhiteSmoke; color:black" align="center"|500 (PDC)<br><b>Frequency:</b>100Hz<br><b>Reverse time:</b> 2µs
|style="background:WhiteSmoke; color:black" align="center"|1.7
|style="background:WhiteSmoke; color:black" align="center"|3.4
|style="background:WhiteSmoke; color:black" align="center"|<b>Ar flow:</b>50sccm<br><b>O<sub>2</sub> flow:</b> 15 sccm
|-
!style="background:silver; color:black;" align="center" |MD PC1 Src6 Pulse DC Upstream
|style="background:LightGrey; color:black" align="center"|<b>ITO</b>
|style="background:WhiteSmoke; color:black" align="center"|3
|style="background:WhiteSmoke; color:black" align="center"|140 (PDC)<br><b>Frequency:</b>100Hz<br><b>Reverse time:</b> 2µs
|style="background:WhiteSmoke; color:black" align="center"|11
|style="background:WhiteSmoke; color:black" align="center"|4.5
|style="background:WhiteSmoke; color:black" align="center"|
|-
!style="background:silver; color:black;" align="center" |MD PC1 Src6 Pulse DC<br> Downstream with reactive O<sub>2</sub>
|style="background:LightGrey; color:black" align="center"|<b>ITO</b>
|style="background:WhiteSmoke; color:black" align="center"|3
|style="background:WhiteSmoke; color:black" align="center"|140 (PDC)<br><b>Frequency:</b>100Hz<br><b>Reverse time:</b> 2µs
|style="background:WhiteSmoke; color:black" align="center"|11.3
|style="background:WhiteSmoke; color:black" align="center"|-
|style="background:WhiteSmoke; color:black" align="center"|<b>Ar flow:</b>50sccm<br><b>O<sub>2</sub> flow:</b> 2 sccm
|-
!style="background:silver; color:black;" align="center" |MD PC1 Src1 RF Upstream
|style="background:LightGrey; color:black" align="center"|<b>Si</b>
|style="background:WhiteSmoke; color:black" align="center"|3
|style="background:WhiteSmoke; color:black" align="center"|120 (RF)
|style="background:WhiteSmoke; color:black" align="center"|1.8
|style="background:WhiteSmoke; color:black" align="center"|-
|style="background:WhiteSmoke; color:black" align="center"|
|-
!style="background:silver; color:black;" align="center" |MD PC3 Src1 Pulse DC<br> Downstream with reactive N<sub>2</sub>
|style="background:LightGrey; color:black" align="center"|<b>Al</b>
|style="background:WhiteSmoke; color:black" align="center"|3
|style="background:WhiteSmoke; color:black" align="center"|900 (PDC)<br><b>Frequency:</b>100Hz<br><b>Reverse time:</b> 2µs
|style="background:WhiteSmoke; color:black" align="center"|29
|style="background:WhiteSmoke; color:black" align="center"|3.2
|style="background:WhiteSmoke; color:black" align="center"|<b>Ar flow:</b>50sccm<br><b>O<sub>2</sub> flow:</b> 15 sccm
|-
|}

Revision as of 23:27, 21 March 2020

Feedback to this page: click here

Cluster-based multi-chamber high vacuum sputtering deposition system. View from service room Ax-1.

Cluster-based multi-chamber high vacuum sputtering deposition system is a robotic cluster tool with two deposition chambers sharing the same distribution trasfer station and the load-lock. The equipment has been installed and accepted in clean-room during January 2020. The purpose of the tool is to deposite variety of materials using DC/RF/PulseDC/HIPIMS magnetron sputtering with or without RF substrate bias. In modul A or PC 1 (process chamber 1) it is possible to deposit any materials using 6 x 3” magnetrons sourses with N2 or O2 reactive gases. Modul B or PC 3 (process chamber 3) is dedicated to oxygen free materials - nitrides and metals. It is eqipted with 1 x 4” + 2 x 3” magnetrons and supplied with N2 process gas for reactive deposition. Both chambers allow heating of substrates up to 600 oC. The equipment is located in clean-room A-5 where the user can acces the cassete loader.


Manufacture: Kurt J. Lesker Company

Model: 2017 PRO Line PVD75 thin film deposition cluster system


The user manual, user APV and contact information can be found in LabManager:

Sputter-System Metal-Oxide(PC1)

Sputter-System Metal-Nitride(PC3)


Thin Film group thinfilm@nanolab.dtu.dk is responsible of the equipment

Target/Metal requests should be sent to metal@nanolab.dtu.dk

If you need a training on the machine please send your request to: training@nanolab.dtu.dk.


Sputtering deposition system design

In the graphs below the HfO2 thickness vs. number of cycles for deposition temperatures between 150 oC and 350 oC presented. Results have been obtained for <100> 150 mm Si wafers with native oxide, based on ellipsometry study.

Power suppliy configuration

bla bla

Power Supply ID Type Maximum output power (W) Maximum output voltage (V) Maximum output current (A) Comments


PC1 Power Supply 1 RF 300
PC1 Power Supply 3 DC 500 1000 4
PC1 Power Supply 4 DC 500 1000 4
PC1 Power Supply 5 Pulse DC 2000 800 5

Max frequency: 100kHz
Max reverse time: 10µs

PC1 Power Supply 7 RF (Substrate) 100
PC3 Power Supply 1 RF 300
PC3 Power Supply 2 Pulse DC 2000 800 5

Max frequency: 100kHz
Max reverse time: 10µs

PC3 Power Supply 3 DC to HiPIMS 1500 1000 4

HiPIMS Unit
Time Avg. Power: 1.5kW
Output Peak Voltage:
-1000V nominal,
-1250V tolerant
Output Peak Current:
200A nominal,
400A toleran


PC3 Power Supply 5 DC 500 1000 4


PC3 Power Supply 6 RF (substrate) 100

Sputter-System Metal-Oxide(PC1)

Bla bla

Sputter-System Metal-Nitride(PC3)

bla bla

Bla bla

Distribution Chamber (Genmark robot)

bla bla


Load lock

bla bla bla bla

Bla bla

Process information

Target size Target material Maximum Power density (W/inch2) Maximum Power (W) Maximum Ramp up/down Power (W/s) Comments


3 inch Al 150 1000 10 DC/HiPIMS
Au 100 700 10 DC/HiPIMS
Ag 100 700 10 DC/HiPIMS
Cu 200 1400 10 DC/HiPIMS
Ni 50 350 10 High strengh magnets/DC
Ti 50 350 10 DC/HiPIMS
Ge (Bonded) 20 140 0.3 DC/RF
Si (Unbonded/Bonded) 20 140 0.3 RF


SiO2 (Bonded) 20 140 0.3 RF


ITO (Bonded) 20 140 0.3 RF/PDC


BaTiO3 (Bonded) 20 140 0.3 RF


NbTi 50 350 10 DC
4 inch Al 150 1800 10 DC/HiPIMS









There are in total 76 developed and tested process recipes for general users (48 for PC1 and 28 for PC3). Starting the recipe the user can change te relevant process parameters: power, pressure, reactive gas ratio, rotation speed, substrate bias etc. In addition to the process recipes, there are also recipes for substrate heating and RF cleaning.


Bla bla



Recipe name Target material Pressure (mTorr) Power (W) Deposition rate (nm/min) Uniformity (%)
on 6 inch wafer
Comments


MD PC1 Src1 RF Upstream SiO2 3 140 (RF) 2.3 0.5
MD PC1 Src2 RF Upstream SiO2 3 140 (RF) 2.6 3
MD PC1 Src3 DC Upstream Ni 3 500 (DC) 23.3 2.5
MD PC1 Src4 DC Upstream Cu 3 500 (DC) 52.2 2.2
MD PC1 Src5 DC Upstream Al 3 200 (DC) 7.9 3.2
MD PC1 Src5 Pulse DC
Downstream with reactive O2
Cu 3 500 (PDC)
Frequency:100Hz
Reverse time: 2µs
1.7 3.4 Ar flow:50sccm
O2 flow: 15 sccm


MD PC1 Src6 Pulse DC Upstream ITO 3 140 (PDC)
Frequency:100Hz
Reverse time: 2µs
11 4.5
MD PC1 Src6 Pulse DC
Downstream with reactive O2
ITO 3 140 (PDC)
Frequency:100Hz
Reverse time: 2µs
11.3 - Ar flow:50sccm
O2 flow: 2 sccm
MD PC1 Src1 RF Upstream Si 3 120 (RF) 1.8 -
MD PC3 Src1 Pulse DC
Downstream with reactive N2
Al 3 900 (PDC)
Frequency:100Hz
Reverse time: 2µs
29 3.2 Ar flow:50sccm
O2 flow: 15 sccm