Specific Process Knowledge/Lithography/UVExposure Dose: Difference between revisions

From LabAdviser
Taran (talk | contribs)
Taran (talk | contribs)
No edit summary
Line 105: Line 105:


==Calculating exposure time==
==Calculating exposure time==
In the maskless aligners, the dose is set as a process parameter in the job. In mask aligners, on the other hand, the parameter that is set is the exposure time, i.e. how long the shutter is open during the exposure.
The exposure dose, ''D'' [J/m<sup>2</sup>], is given by:
The exposure dose, ''D'' [J/m<sup>2</sup>], is given by:


Line 172: Line 174:


<br clear="all" />
<br clear="all" />
=Exposure dose when using AZ 351B developer (NaOH)=
==KS Aligner (351B)==
The KS Aligner has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm. Dependent on the spectral sensitivity of the resist, the optimal dose may be increased compared to broadband exposure on the Aligner-6inch. Unless otherwise stated, the exposure doses given here are for standard silicon wafers.
<br clear="all" />
{|border="1" cellspacing="1" cellpadding="7" style="text-align:left;"
|-
|-
|-style="background:silver; color:black"
|
!Thickness
!Dose
![[Specific_Process_Knowledge/Lithography/Development#Developer-6inch|Development]]
!Comments
|-
|-
|-style="background:WhiteSmoke; color:black"
!rowspan="3"|AZ 5214E
|1.5 µm
|65-75mJ/cm<sup>2</sup>
|60 s
|rowspan="3"|Positive process
|-style="background:WhiteSmoke; color:black"
|2.2 µm
|64-80 mJ/cm<sup>2</sup>
|70 s
|-style="background:WhiteSmoke; color:black"
|4.2 µm
|~160 mJ/cm<sup>2</sup>
|3 minutes
|-
|-
|-style="background:LightGrey; color:black"
!rowspan="2"|AZ 5214E
|1.5 µm
|30 mJ/cm<sup>2</sup>
|60 s
|rowspan="2"|Image reversal process.
Reversal bake: 100s at 110°C.<br>Flood exposure after reversal bake: 210 mJ/cm<sup>2</sup>
|-style="background:LightGrey; color:black"
|2.2 µm
|35 mJ/cm<sup>2</sup>
|70 s
|-
|-
|-style="background:WhiteSmoke; color:black"
!AZ 4562
|10 µm
|~320 mJ/cm<sup>2</sup>
|5 minutes
|Multiple exposure with 10 s pauses is recommended.
|-
|}
<br clear="all" />
'''Additional information:'''
'''AZ 5214E image reversal'''
*1.5 µm resist on boron glass: around 49 mJ/cm<sup>2</sup> (supplied March 2013 by Morten Bo Lindholm Mikkelsen, DTU Nanotech).


=Exposure dose when using AZ 726 MIF developer (TMAH)=
=Exposure dose when using AZ 726 MIF developer (TMAH)=
Line 417: Line 353:


Aligner: Maskless 03 uses a 405nm laser diode array source. Information about the process parameters for exposure using Aligner: Maskless 03 can be found [[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_03_processing#Process_Parameters|'''here''']]. The process log is also a good source of information.
Aligner: Maskless 03 uses a 405nm laser diode array source. Information about the process parameters for exposure using Aligner: Maskless 03 can be found [[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_03_processing#Process_Parameters|'''here''']]. The process log is also a good source of information.
=Exposure dose when using AZ 351B developer (NaOH)=
==KS Aligner (351B)==
The KS Aligner has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm. Dependent on the spectral sensitivity of the resist, the optimal dose may be increased compared to broadband exposure on the Aligner-6inch. Unless otherwise stated, the exposure doses given here are for standard silicon wafers.
<br clear="all" />
{|border="1" cellspacing="1" cellpadding="7" style="text-align:left;"
|-
|-
|-style="background:silver; color:black"
|
!Thickness
!Dose
![[Specific_Process_Knowledge/Lithography/Development#Developer-6inch|Development]]
!Comments
|-
|-
|-style="background:WhiteSmoke; color:black"
!rowspan="3"|AZ 5214E
|1.5 µm
|65-75mJ/cm<sup>2</sup>
|60 s
|rowspan="3"|Positive process
|-style="background:WhiteSmoke; color:black"
|2.2 µm
|64-80 mJ/cm<sup>2</sup>
|70 s
|-style="background:WhiteSmoke; color:black"
|4.2 µm
|~160 mJ/cm<sup>2</sup>
|3 minutes
|-
|-
|-style="background:LightGrey; color:black"
!rowspan="2"|AZ 5214E
|1.5 µm
|30 mJ/cm<sup>2</sup>
|60 s
|rowspan="2"|Image reversal process.
Reversal bake: 100s at 110°C.<br>Flood exposure after reversal bake: 210 mJ/cm<sup>2</sup>
|-style="background:LightGrey; color:black"
|2.2 µm
|35 mJ/cm<sup>2</sup>
|70 s
|-
|-
|-style="background:WhiteSmoke; color:black"
!AZ 4562
|10 µm
|~320 mJ/cm<sup>2</sup>
|5 minutes
|Multiple exposure with 10 s pauses is recommended.
|-
|}
<br clear="all" />
'''Additional information:'''
'''AZ 5214E image reversal'''
*1.5 µm resist on boron glass: around 49 mJ/cm<sup>2</sup> (supplied March 2013 by Morten Bo Lindholm Mikkelsen, DTU Nanotech).

Revision as of 10:28, 20 March 2020

Feedback to this page: click here

Exposure dose

Spectral sensitivity of AZ resists represented as optical absorption. From http://www.microchemicals.com/

During exposure of the resist, the photoinitiator, or photo-active component, reacts with the exposure light, and starts the reaction that makes the resist develop in the developer. In a positive resist, it makes the resist become soluble in the developer. In a negative resist, usually assisted by thermal energy in the post-exposure bake, it makes the resist insoluble in the developer. The amount of light required to fully develop the resist in the development process, is the exposure dose. The optimal exposure dose is a function of many parameters, including the type of resist, the resist thickness, and the sensitivity of the resist.

The resist sensitivity is a measure of how efficiently it reacts to the exposure light. Spectral sensitivity is the sensitivity of the resist as a function of wavelength. It is usually given simply as the range from the wavelength below which absorption in the resist material makes lithography impractical to the wavelength at which the photoinitiator is no longer efficiently activated. The spectral sensitivity is listed in the Resist Overview. Within this range, the optical absorption is commonly used as a measure of sensitivity. A high absorption coefficient signifies a high sensitivity, as the light is absorbed by the photoinitiator. Because of spectral sensitivity, the optimal dose of a given resist type and thickness is also a function of the spectral distribution of the exposure light, i.e. the equipment used for the exposure, see tables below. Using a combination of experience, calculation, and assumption, one may be able to estimate the dose for one equipment from the known dose on another equipment.

Due to reflection and refraction at the interface between the resist and the substrate, the optimal dose may also be a function of the type of substrate used. Unless otherwise stated, the exposure doses given here are for standard silicon wafers.

Apart from the already mentioned factors, the optimal dose also depends on the developer chemistry and the parameters used in the development process. Finally, the requirements to the lithographic process in terms of resolution, bias (line broadening), etch selectivity, side wall angle, etc. may narrow down, or widen, the process window. The exposure doses given in the sections below should be used as a starting point for individual fabrication process development.

Due to the process of bleaching, where the absorption of the resist changes during exposure, the exposure dose is unfortunately not always constant at different intensities of the exposure light. The exposure time is thus not always a linear function of the exposure intensity.


Mask aligners:

Lamp Installed filter Adjusted intensity Filter options
KS Aligner 350 W Hg i-line notch filter

365nm (FWHM = 7 nm)

8 mW/cm2 @ 365 nm (Constant Intensity)
  • no filter (broadband)
  • 313 nm (notch)
  • 303 nm (notch)
Aligner: MA6 - 2 500 W Hg-Xe i-line notch filter

365nm (FWHM = ? nm)

The intensity is set by the user

11 mW/cm2 @ 365 nm

  • no filter (broadband)
  • UV400 (350 - 400 nm)
  • UV350 (280 - 350 nm)
  • UV250 (240 - 260 nm)

The most powerful UV lines in the Hg spectrum are the i-, h-, and g-lines at 356 nm, 405 nm, and 435 nm wavelength, respectively. While the Hg lamp produces little or no intensity in the deep-UV (UV-C) range, the Hg-Xe lamp has increased output below 300 nm.


Maskless aligners:

Source Wavelength
Aligner: Maskless 01 LED 365nm
Aligner: Maskless 02 Laser diode array 375nm

or

405nm

Aligner: Maskless 03 Laser diode array 405nm


Calculating exposure time

In the maskless aligners, the dose is set as a process parameter in the job. In mask aligners, on the other hand, the parameter that is set is the exposure time, i.e. how long the shutter is open during the exposure.

The exposure dose, D [J/m2], is given by:

D = I x t ,

where I [W/m2] is the intensity of the exposure light, and t [s] is the exposure time. As the intensity is specific to the spectral sensitivity of the sensor used to measure the exposure light, and the exposure time is specific to the spectral distribution of the exposure light (cf. spectral sensitivity), this dose is specific to the combination of exposure source and optical sensor.

Given the optimum exposure dose, the exposure time is calculated as:

t = D / I .

It is important to keep in mind that this exposure time is valid only for a specific combination of exposure source and optical sensor, as well as for a specific development process.



Exposure dose when using AZ 726 MIF developer (TMAH)

KS Aligner

The KS Aligner has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm. Unless otherwise stated, the exposure doses given here are for standard silicon wafers.


Thickness Dose Development Comments
AZ 5214E 1.5 µm 72 mJ/cm2 Single puddle, 60 s Positive process
2.2 µm 80 mJ/cm2
4.2 µm 160 mJ/cm2
AZ 4562 10 µm 480-540 mJ/cm2 Multiple puddle, 4 x 60 s Multiple exposure with 10-15 s pauses is recommended.
AZ MiR 701 1 µm ~180 mJ/cm2 Single puddle, 60 s PEB: 60 s at 110°C

Preliminary results

2 µm ~200 mJ/cm2 Single puddle, 60 s
4 µm ~400 mJ/cm2 Single puddle, 60 s PEB: 90 s at 110°C

Preliminary results

AZ nLOF 2020 2 µm 100-120 mJ/cm2 Single puddle, 60 s PEB: 60 s at 110°C

Side wall angle ~15°. For lover angle, develop 30 s (~5°)


Aligner: MA6 - 2

The Aligner: MA6-2 has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm. Unless otherwise stated, the exposure doses given here are for standard silicon wafers.


Thickness Dose Development Comments
AZ 5214E 1.5 µm 72 mJ/cm2 Single puddle, 60 s Positive process
2.2 µm 90 mJ/cm2 Single puddle, 60 s
AZ 5214E 1.5 µm 22? mJ/cm2 Single puddle, 60 s Image reversal process.

Reversal bake: 120s at 110°C.
Flood exposure after reversal bake: 195 mJ/cm2

2.2 µm 25 mJ/cm2 Single puddle, 60 s
AZ 4562 10 µm 520-?? mJ/cm2 Multiple puddle, 4 x 60 s Multiple exposure with 10 s pauses is recommended.

Process not yet established.

AZ MiR 701 1.5 µm 169 mJ/cm2 Single puddle, 60 s PEB: 60 s at 110°C
2 µm ~200 mJ/cm2 Single puddle, 60 s
4 µm ~280 mJ/cm2 Single puddle, 60 s PEB: 60 s at 110°C

Process adopted from process logs.

AZ nLOF 2020 1.5 µm 104 mJ/cm2 Single puddle, 30 s PEB: 60 s at 110°C

Use 60 s development for lift-off


Maskless aligners

THIS SECTION IS UNDER CONSTRUCTION

Aligner: Maskless 01

Aligner: Maskless 01 uses a 365nm LED source. The exposure dose needed seems to follow the dose needed to process the same substrate in Aligner: MA6-2. As doses get higher, there is a tendency for the dose needed in the Aligner: Maskless 01 to exceed the dose needed in Aligner: MA6-2.

More information about the process parameters for exposure using Aligner: Maskless 01 can be found here. The process log is also a good source of information.

Aligner: Maskless 02

Aligner: Maskless 02 uses a 375nm or 405nm laser diode array source. Information about the process parameters for exposure using Aligner: Maskless 02 can be found here. The process log is also a good source of information.

Aligner: Maskless 03

Aligner: Maskless 03 uses a 405nm laser diode array source. Information about the process parameters for exposure using Aligner: Maskless 03 can be found here. The process log is also a good source of information.

Exposure dose when using AZ 351B developer (NaOH)

KS Aligner (351B)

The KS Aligner has an i-line notch filter installed. This results in an exposure light peak around 365 nm with a FWHM of 7 nm. Dependent on the spectral sensitivity of the resist, the optimal dose may be increased compared to broadband exposure on the Aligner-6inch. Unless otherwise stated, the exposure doses given here are for standard silicon wafers.


Thickness Dose Development Comments
AZ 5214E 1.5 µm 65-75mJ/cm2 60 s Positive process
2.2 µm 64-80 mJ/cm2 70 s
4.2 µm ~160 mJ/cm2 3 minutes
AZ 5214E 1.5 µm 30 mJ/cm2 60 s Image reversal process.

Reversal bake: 100s at 110°C.
Flood exposure after reversal bake: 210 mJ/cm2

2.2 µm 35 mJ/cm2 70 s
AZ 4562 10 µm ~320 mJ/cm2 5 minutes Multiple exposure with 10 s pauses is recommended.


Additional information:

AZ 5214E image reversal

  • 1.5 µm resist on boron glass: around 49 mJ/cm2 (supplied March 2013 by Morten Bo Lindholm Mikkelsen, DTU Nanotech).