Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/polySi/Cduv: Difference between revisions
Appearance
No edit summary |
No edit summary |
||
| Line 23: | Line 23: | ||
| Pegasus/jmli | | Pegasus/jmli | ||
| 10 minute TDESC clean + 45 sec barc etch | | 10 minute TDESC clean + 45 sec barc etch | ||
| | | nanolab/jml/showerhead/polySi etch DUV mask, 20 cycles or 3:02 minutes | ||
| S004675 | | S004675 | ||
! Old showerhead | ! Old showerhead | ||
| Line 41: | Line 41: | ||
| Pegasus/jmli | | Pegasus/jmli | ||
| 10 minute TDESC clean + 45 sec barc etch | | 10 minute TDESC clean + 45 sec barc etch | ||
| | | nanolab/jml/showerhead/polySi etch DUV mask, 20 cycles or 3:02 minutes | ||
| S004675 | | S004675 | ||
! New showerhead | ! New showerhead | ||
Revision as of 22:23, 25 November 2019
| Date | Substrate Information | Process Information | SEM Images | ||||||
|---|---|---|---|---|---|---|---|---|---|
| Wafer info | Mask | Material/ Exposed area | Tool / Operator | Conditioning | Recipe | Wafer ID | Comments | ||
| 20/11-2014 | 6" Wafer with 210 nm oxide and 1800 nm polysilicon | standard stepper mask (50 nm barc + 320 nm krf) | Si / 50+ % | Pegasus/jmli | 10 minute TDESC clean + 45 sec barc etch | nanolab/jml/showerhead/polySi etch DUV mask, 20 cycles or 3:02 minutes | S004675 | Old showerhead | |
| 1/12-2014 | 1/4 6" Wafer with 210 nm oxide and 1800 nm polysilicon crystalbonded on carrier | standard stepper mask (50 nm barc + 320 nm krf) | Si / 50+ % | Pegasus/jmli | 10 minute TDESC clean + 45 sec barc etch | nanolab/jml/showerhead/polySi etch DUV mask, 20 cycles or 3:02 minutes | S004675 | New showerhead | |