Jump to content

Specific Process Knowledge/Etch/ICP Metal Etcher/silicon nitride: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
Jmli (talk | contribs)
No edit summary
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/silicon_nitride click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/silicon_nitride click here]'''  





Revision as of 21:37, 25 November 2019

Feedback to this page: click here


Slow etch of silicon nitride with resist as masking material - on 6" carrier wafer with recess

This recipe can be used for slow etching of silicon nitride with resist as masking material. Here are some test results presented. The same recipe is being used for SiO2, see the result for that here


Parameter A slow etch with carrier
Coil Power [W] 200
Platen Power [W] 25
Platen temperature [oC] 0
CF4 flow [sccm] 20
H2 flow [sccm] 10
Pressure [mTorr] 3


Results Test on wafer with 20% load, by Izzet Yildiz @Nanotech Test by BGHE @danchip
Etch rate of LPCVD nitride 60-65 nm/min (20% etch load) (Feb. 2014)  
Selectivity to resist [SiN : AZ resist] 1:0.75  
Wafer uniformity (100mm) ?  
Profile [o] ?  
Wafer uniformity map (click on the image to view a larger image) not measured  
SEM profile images Not measured  
Etch rate in Barc   ~50 nm/min (Date: 2014-09-09)
Etch rate in KRF resist   ~40 nm/min (Date: 2014-09-09)