Descum of AZ  Mir 701 resist on 100mm silicon wafer. Five wafers were placed vertically in chamber.


Flow of O2 was 100
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  

Revision as of 16:57, 19 November 2019

Feedback to this page: click here

Descum results

Plasma asher 1

Descum results plasma asher 1
Descum results plasma asher 2

Descum of AZ5214E resist on 50mm silicon wafer. Wafer was placed horisontally in chamber on a 100 mm carier wafer.

Note: Plasma asher was cold before use

Settings Etched Thickness (nm)
ashing time (min)
Recipe O2 flow N2 flow Power 1 2 5 7 10 10
1 70 70 150 14,2 16,3 47,6 123,2 854,3 862,1
2 500 0 200 8,1 32,9 271,1 495,6 446,2


Conny Hjort & Jesper Hanberg September 2019



Plasma asher 2

Descum of AZ Mir 701 resist on 100mm silicon wafer. Five wafers were placed vertically in chamber.

Flow of O2 was 100

Ashing time (min) 1 2 3 4 6 7 8 9 10 12 14 15 20
Etched Thickness (nm) 8,7 5,1 12,5 6,2 31,8 86,0 25,7 46,8 38,3 49,7 59,4 140,1 360,7