Jump to content

Specific Process Knowledge/Back-end processing/Disco Saw: Difference between revisions

From LabAdviser
Jehan (talk | contribs)
Jehan (talk | contribs)
Line 4: Line 4:
The dicer feature versatile processing capabilities, compact designs, and high precision and reliability. Users perform workpiece loading, alignment, and unloading manually.
The dicer feature versatile processing capabilities, compact designs, and high precision and reliability. Users perform workpiece loading, alignment, and unloading manually.


The dicer at DANCHIP is placed in room 157 on the first floor in bldg. 346. Please notice that this is not a cleanroom and that the dicing process is very dirty. Think about how to clean your samples if you want to bring them back in the cleanroom.
The dicer at DTU Nanolab is placed in room 157 on the first floor in bldg. 346. Please notice that this is not a cleanroom and that the dicing process is very dirty. Think about how to clean your samples if you want to bring them back in the cleanroom.




Line 14: Line 14:
<!-- give the link to the equipment info page in LabManager: -->
<!-- give the link to the equipment info page in LabManager: -->
[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=168 Saw in LabManager]
[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=168 Saw in LabManager]


== Process information ==
== Process information ==

Revision as of 10:06, 6 August 2019

Feedback to this page: click here

Disco Automatic dicing saw, model DAD321

The dicer feature versatile processing capabilities, compact designs, and high precision and reliability. Users perform workpiece loading, alignment, and unloading manually.

The dicer at DTU Nanolab is placed in room 157 on the first floor in bldg. 346. Please notice that this is not a cleanroom and that the dicing process is very dirty. Think about how to clean your samples if you want to bring them back in the cleanroom.


The user manual, user APV, technical information and contact information can be found in LabManager:

Dicer positioned on 1. floor bldg 346 room 157

Saw in LabManager

Process information


Overview of the performance Disco DAD321 Dicer

Purpose Equipment for dicing out samples
  • Pure Silicon samples
  • Silicon bonded to Silicon
  • Silicon bonded to Pyrex/Borofloat
  • Pyrex/Borofloat
Performance X-axis cutting range

192 mm

X-axis cut speed

0.1 - 300 mm/sec

Y-axis cutting range

162 mm

Y-axis index step

0.0002 mm

Y-axis single error

0.003 or less

Hardware settings Maximum blade size

ø76.2 mm

Substrates Substrate size

up to 6"

Layers that can't be diced
  • Thick metal (>0.75 mm)
  • III-V samples



Comparing dicing parameters for different materials

Silicon Pyrex or bonded Si/Pyrex
Bladetype HUB Blade ZH05 (27HEEF) HUBless Blade B1A862
Blade width 50 µm 150 µm
Cutlinewidth 60 µm 180 - 200 µm
Recommended feed speed Up to 20 mm/sec Up to 2 mm/sec (0.5 mm/sec)
Recommended dice depth Set blade height to 200µm (preferred).
This leaves 125µm uncut since blue tape is 75µm.
It is possible to cut through the sample.
Set blade height to 200µm (preferred).
This leaves 125µm uncut since blue tape is 75µm.
It is possible to cut through the sample.
Max. sample thickness 1.5 mm 2.0 mm

Images of diced samples

Si V-groove diced with ZH05 blade