Specific Process Knowledge/Etch/ICP Metal Etcher/silicon nitride: Difference between revisions
Appearance
No edit summary |
|||
| Line 3: | Line 3: | ||
===Slow etch of silicon nitride with resist as masking material - on 6" carrier wafer with recess === | ===Slow etch of silicon nitride with resist as masking material - on 6" carrier wafer with recess === | ||
This recipe can be used for slow etching of silicon nitride with resist as masking material. Here are some test results presented. | This recipe can be used for slow etching of silicon nitride with resist as masking material. Here are some test results presented. The same recipe is being used for SiO2, see the result for that here: [Specific Process Knowledge/Etch/ICP Metal Etcher/silicon oxide/ | ||
Page | |||
Discussion | |||
Edit | |||
History | |||
Delete | |||
Move | |||
Protect | |||
{| border="2" cellspacing="2" cellpadding="3" | {| border="2" cellspacing="2" cellpadding="3" | ||
Revision as of 08:01, 26 June 2019
Feedback to this page: click here
Slow etch of silicon nitride with resist as masking material - on 6" carrier wafer with recess
This recipe can be used for slow etching of silicon nitride with resist as masking material. Here are some test results presented. The same recipe is being used for SiO2, see the result for that here: [Specific Process Knowledge/Etch/ICP Metal Etcher/silicon oxide/
Page
Discussion
Edit
History
Delete
Move
Protect
| Parameter | A slow etch with carrier |
|---|---|
| Coil Power [W] | 200 |
| Platen Power [W] | 25 |
| Platen temperature [oC] | 0 |
| CF4 flow [sccm] | 20 |
| H2 flow [sccm] | 10 |
| Pressure [mTorr] | 3 |
| Results | Test on wafer with 20% load, by Izzet Yildiz @Nanotech | Test by BGHE @danchip |
|---|---|---|
| Etch rate of LPCVD nitride | 60-65 nm/min (20% etch load) (Feb. 2014) | |
| Selectivity to resist [SiN : AZ resist] | 1:0.75 | |
| Wafer uniformity (100mm) | ? | |
| Profile [o] | ? | |
| Wafer uniformity map (click on the image to view a larger image) | not measured | |
| SEM profile images | Not measured | |
| Etch rate in Barc | ~50 nm/min (Date: 2014-09-09) | |
| Etch rate in KRF resist | ~40 nm/min (Date: 2014-09-09) |