*5206E 0.5µm 375nm (fast + quality)
*5206E 0.5µm 375nm, dev SP30s
Fast: 60mJ/cm<sup>2</sup>; defoc -6 (not optimized)
Fast: 60mJ/cm<sup>2</sup>; defoc -6 (1µm, not optimized)
Quality: 60mJ/cm<sup>2</sup>; defoc -6 (not optimized)
 
*5214E 1.5µm 405nm (fast)
Quality: 60mJ/cm<sup>2</sup>; defoc -6 (~750nm, not optimized)
Fast: 90mJ/cm<sup>2</sup>; defoc -2
*5214E 1.5µm 405nm, dev SP60s
*5214E 1.5µm 375nm (fast + quality)
Fast: 90mJ/cm<sup>2</sup>; defoc -2 (1-2µm)
Fast: 65mJ/cm<sup>2</sup>; defoc 2
*5214E 1.5µm 375nm, dev SP60s
Quality: 65mJ/cm<sup>2</sup>; defoc 2
Fast: 65mJ/cm<sup>2</sup>; defoc 2 (~1µm)
*MiR 701 1.5µm 405nm (fast)
 
*MiR 701 1.5µm 375nm (fast + quality)
Quality: 65mJ/cm<sup>2</sup>; defoc 2 (~750nm)
*nLOF 2020 2µm 375nm (fast + quality)
*MiR 701 1.5µm 405nm, PEB 60s@110°C dev SP60s
Fast: 200mJ/cm<sup>2</sup>; defoc -5 (~1µm, not optimized)
*MiR 701 1.5µm 375nm, PEB 60s@110°C dev SP60s
Fast: 170mJ/cm<sup>2</sup>; defoc -5 (1µm)
 
Quality: 180mJ/cm<sup>2</sup>; defoc -6 (750nm)
*nLOF 2020 2µm 375nm, PEB 60s@110°C dev SP60s
Fast: 400mJ/cm<sup>2</sup>; defoc 5 (~1µm, not optimized)
 
Quality: 400mJ/cm<sup>2</sup>; defoc 0 (1µm)


*Substrate centering + flat alignment test
*Substrate centering + flat alignment test

Revision as of 13:02, 22 March 2019

Feedback to this page: click here

THIS PAGE IS UNDER CONSTRUCTION

Exposure technology

Aligner: Maskless 02 is not a direct writer. In the maskless aligner, the exposure light is passed through a spatial light modulator, much like in a video projector, and projected onto the substrate, thus exposing an area of the design at a time. The substrate is exposed by scanning the exposure field across the substrate in a succession of stripes.

The light source is a laser diode (array) with a wavelength of 375nm (2.8W) or 405nm (8W). The spacial light modulator is a digital micro-mirror device. The individual mirrors of the DMD are switched in order to represent the design, and the laser is flashed in order to yield the desired exposure dose. This image is projected onto the substrate through a lens(system). The projected image yields a pixel size of 160nm X 160nm at wafer scale. The image is scanned across the substrate, in order to expose the entire design, each stripe overlapping (2 or 4 times) in order to minimize uniformity effects and stitching errors.

The writing head of the Aligner: Maskless 02 moves only in the z-direction. Using an optical (or pneumatic) focusing system, the maskless aligner is able to do real-time autofocus. The defocus process parameter is used to compensate offsets in the focusing mechanism, and to optimize printing quality in different resists and varying thicknesses. The stage of the Aligner: Maskless 02 moves only in x and y. It has no theta-axis. All rotation during alignment is thus accomplished by transformation of the input design.

Process Parameters

  • 5206E 0.5µm 375nm, dev SP30s

Fast: 60mJ/cm2; defoc -6 (1µm, not optimized)

Quality: 60mJ/cm2; defoc -6 (~750nm, not optimized)

  • 5214E 1.5µm 405nm, dev SP60s

Fast: 90mJ/cm2; defoc -2 (1-2µm)

  • 5214E 1.5µm 375nm, dev SP60s

Fast: 65mJ/cm2; defoc 2 (~1µm)

Quality: 65mJ/cm2; defoc 2 (~750nm)

  • MiR 701 1.5µm 405nm, PEB 60s@110°C dev SP60s

Fast: 200mJ/cm2; defoc -5 (~1µm, not optimized)

  • MiR 701 1.5µm 375nm, PEB 60s@110°C dev SP60s

Fast: 170mJ/cm2; defoc -5 (1µm)

Quality: 180mJ/cm2; defoc -6 (750nm)

  • nLOF 2020 2µm 375nm, PEB 60s@110°C dev SP60s

Fast: 400mJ/cm2; defoc 5 (~1µm, not optimized)

Quality: 400mJ/cm2; defoc 0 (1µm)

  • Substrate centering + flat alignment test

Exposure dose

Defocus

Exposure mode

(high quality, fast)


High Aspect Ratio mode

  • Intensity vs. aperture (405nm + 375nm)
  • Dose test for 1.5µm MiR (405nm + 375nm)

Writing speed

  • Speed vs. area (375nm)
    • Online
    • Offline
The writing speed of Aligner: Maskless 02 as a function of the exposure area


  • Speed vs. dose (375nm + 405nm)
The writing speed of Aligner: Maskless 01 as a function of the exposure dose



Resolution

Substrate centring and flat alignment

During substrate detection, the sample is scanned along the X- and Y-axes, as well as diagonally. From these measurements, the size (diameter) of the substrate is calculated, as well as the stage position matching the center of the substrate. This stage position will be the default origin for the subsequent exposure.

At the end of substrate detection, the sample is scanned twice along the bottom edge (flat), in order to determine the substrate rotation. This angle will be presented in the exposure panel along with the option to expose the design rotated in order to compensate for this angle, i.e. aligned to the flat/edge of the substrate.

Labelling

labelfile.lbl (tab-delimited ASCII file).

X | Y | UNIT | HEIGHT | UNIT | TITLE

-16000 | -46000 | um | 2000 | um | TARAN DTU Nanolab 20190320

This produces a 2mm high, approximately 32mm long wafer ID at the flat of a 4" wafer.

Some special characters are not allowed (e.g. ';').

Alignment

Top Side Alignment

  • 4 marks (before final installation)
  • Scaling (375nm, high res camera)

Back Side Alignment

Advanced Field alignment (TSA)

  • 4 marks, 25 fields (375nm, high res camera)