The titanium Ti2p peak is notoriously difficult to fit. From [[Specific Process Knowledge/Characterization/XPS/Processing/XPSknowledgeview |XPS Knowledge view]] we have:
The titanium Ti2p peak is notoriously difficult to fit. From [[Specific Process Knowledge/Characterization/XPS/Processing/XPSknowledgeview |XPS Knowledge view]] we have:
'''''Binding energies of common chemical states'''''
{| class="wikitable"
|-
! ''Chemical state'' !!'' Binding energy Ti2p<sub>3/2</sub>/eV''
|-
| ''Ti metal'' || ''454.1''
|-
| ''TiN'' || 545.9
|-
| ''TiO<sub>2</sub></sub>'' || ''458.5''
|-
| ''SrTiO<sub>2</sub>'' || ''458.4''
|-
|}
'''''Interpretations of XPS spectra'''''


*'' Ti metal gives asymmetric Ti2p peak shapes''