The titanium Ti2p peak is notoriously difficult to fit. From [[Specific Process Knowledge/Characterization/XPS/Processing/XPSknowledgeview |XPS Knowledge view]] we have:
The titanium Ti2p peak is notoriously difficult to fit. From [[Specific Process Knowledge/Characterization/XPS/Processing/XPSknowledgeview |XPS Knowledge view]] we have:


{|
 
|-
 
|* Ti metal gives asymmetric Ti2p peak shapes
''* Ti metal gives asymmetric Ti2p peak shapes
|-
 
|** TiO<sub>2</sub> has symmetric peak shapes and TiN has complex peak shape, involving satellite features.
** TiO<sub>2</sub> has symmetric peak shapes and TiN has complex peak shape, involving satellite features.
|-
 
|*Ti2p peak has significantly split spin-orbit components (Δ<sub>metal</sub>=6.1 eV)
*Ti2p peak has significantly split spin-orbit components (Δ<sub>metal</sub>=6.1 eV)
|-
 
|** Splitting Δ-value varies with chemical state (Δ<sub>nitride</sub>=6.0 eV,Δ<sub>oxide</sub>=5.7 eV).
** Splitting Δ-value varies with chemical state (Δ<sub>nitride</sub>=6.0 eV,Δ<sub>oxide</sub>=5.7 eV).
|-
 
|** Typically FWHM for each spin-orbit component is the same, but for Ti2p the Ti2p<sub>1/2</sub> component is much broader than the Ti2p<sub>3/2</sub> peak.
** Typically FWHM for each spin-orbit component is the same, but for Ti2p the Ti2p<sub>1/2</sub> component is much broader than the Ti2p<sub>3/2</sub> peak.
|-
 
|*** Consequently, Ti2p<sub>1/2</sub> peak is much shorter than expected.
*** Consequently, Ti2p<sub>1/2</sub> peak is much shorter than expected.
|-
 
|*** Caused by Coster-Kronig effect. (Post-ionization, Ti2p<sub>1/2</sub> is very short lived compared to Ti2p<sub>3/2</sub> state.)
*** Caused by Coster-Kronig effect. (Post-ionization, Ti2p<sub>1/2</sub> is very short lived compared to Ti2p<sub>3/2</sub> state.)
|-
 
|*** Causes difficulty in accurately peak fitting Ti2p region with multiple chemical states.
*** Causes difficulty in accurately peak fitting Ti2p region with multiple chemical states.''
|-
|}