Specific Process Knowledge/Thin film deposition/Deposition of Silicon Nitride/Deposition of Silicon Nitride using PECVD: Difference between revisions
| Line 5: | Line 5: | ||
== Deposition of SiN with PECVD4 == | == Deposition of SiN with PECVD4 == | ||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality Controle (QC) for PECVD4''' | |||
|- | |||
| | |||
*[http://labmanager.danchip.dtu.dk/d4Show.php?id=1402&mach=106 The QC procedure for PECVD3]<br> | |||
*[http://www.labmanager.danchip.dtu.dk/view_binary.php?type=data&mach=106 The newest QC data for PECVD3]<br> | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:200px" | |||
! QC Recipe: | |||
! QCNITRIDE | |||
|- | |||
| SiH<sub>4</sub> flow | |||
|30 sccm | |||
|- | |||
|NH<sub>3</sub> flow | |||
|30 sccm | |||
|- | |||
|N<sub>2</sub> flow | |||
|1470 sccm | |||
|- | |||
|Pressure | |||
|845 mTorr | |||
|- | |||
|RF-power | |||
| | |||
*HF: 100 W 7.8s | |||
*LF: 100 W 2.2s | |||
|- | |||
|} | |||
| align="center" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px" | |||
!QC limits | |||
!PECVD3 | |||
|- | |||
|Depoition rate | |||
|~40 nm/min | |||
|- | |||
|Non-uniformity | |||
|<3.0 % | |||
|- | |||
|Refractive Index | |||
|2.02 - 2.04 | |||
|} | |||
|- | |||
|} | |||
|} | |||
{| border="1" cellspacing="2" cellpadding="2" | {| border="1" cellspacing="2" cellpadding="2" | ||
Revision as of 15:42, 17 October 2018
Feedback to this page: click here
At the moment DANCHIP has 2 PECVDs that can deposite silicon nitride and silicon oxynitride. PECVD4 is for clean silicon based and III-V based samples. PECVD3 is for silicon based samples but here up 5% (4 cm2) wafer coverage of other materials as metals are allowed. Look at the PECVD page to learn more about the PECVDs at DANCHIP. All though PECVD3 and PECVD4 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.
Deposition of SiN with PECVD4
| Quality Controle (QC) for PECVD4 | ||||||||||||||||||||||
|
| Recipe | Dep. rate [nm/min] | RI | Unif. [%] | Stress [MPa] | Comments | SiH4 [sccm] | NH3 [sccm] | N2O [sccm] | N2 [sccm] | Pressure [mTorr] | Power [W] | Load | Tune | Time [mm:ss] | Tested
|
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| MF SIN | 12.9-13.0 nm/min | 2.038-2.044 | ± 1.7% | 157 MPa | more results | 40 | 40 | 1920 | 900 mTorr | 20HF6"/20LF2" | 10:00/60:00(stress) | February 2017 bghe | |||
| LF SIN | 40-43 nm/min | 1.983-1.984 | ± 3.9-4.4% | Compressive: 565.4 MPa | 40 | 20 | 1960 | 550 mTorr | 60LF | 2:00/23:00(stress) | February 2017 bghe | ||||
| HF SiN | 12.2-12.4 nm/min | 2.017-2.021 | ± 1.2-1.6% | Tensile: 431.6 MPa | 40 | 55 | 1960 | 900 mTorr | 20 W | 10:00/56:00(stress) | February 2017 bghe |
Recipes on PECVD3 for deposition of silicon nitride and silicon oxynitride
| Quality Controle (QC) for PECVD3 | ||||||||||||||||||||||
|
Recipes
| Recipe name | SiH4 flow [sccm] | NH3 flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| MFSiNLS2 | 30 | 30 | 1470 | 845 | 100HF 7.8s
100LF 2.2s |
Low stress nitride - standard recipe. The latest measured values can be seen in the process control sheet in LabManager. |
| MFSiNLS | 30 | 30 | 1470 | 650 | 20HF 6s
30LF 2s |
Low stress nitride - old standard recipe. This one is not running well any more. |
| LFSiN | 30 | 15 | 1470 | 550 | 60LF | Compressive stress |
| HFSiN | 30 | 42 | 1470 | 900 | 20HF | Tensile stress |
LF=Low Frequency HF=High Frequency MF=Mixed Frequency SiN=Silicon Nitride LS=Low Stress
Expected results
| Recipe name | Deposition rate [Å/min] | RI | Uniformity [%] [Std./mean] |
Stress [MPa] | KOH etch rate [Å/min] | BHF etch rate [Å/min] | See more |
| MFSiNLS2 | ~422 (bghe Feb 2016) | ~2.03 | ~2 | ~6 (bghe Feb 2016) | ~2.1 (bghe Feb 2016) | ~? | see DOE |
| MFSiNLS | ~107 | ~1.99 | ~4 | ~-30 | ~2.5 | ~250 | . |
| LFSiN | ~550 | ~1.96 | ~3 | ~-630 | . | . | . |
| HFSiN | ~130 | ~1.97 | ~2 | ~460 | . | . | . |
Recipes on PECVD2 for deposition of silicon nitride and silicon oxynitride
Recipes
| Recipe name | SiH4 flow [sccm] | NH3 flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| SINSTD80 | 30 | 20 | 1000 | 500 | 80 | |
| SINSTD96 | 30 | 20 | 1000 | 500 | 96 | |
| 1SiN | 40 | 20 | 1000 | 700 | 150 |
Expected results
| Recipe name | Deposition rate [nm/min] | RI | Uniformity [%] | Stress [MPa] | BHF etch rate [Å/min] | Comments |
| 1SiN |
Deposition rate in the middle of two wafers: 49nm/min+-1nm/min (2015-04-24 BGHE) |
~2-4% (2015-04-24 BGHE) |
||||
| SINSTD80 | 68nm/min (2014-07-07 JML)- unstable deposition rate | |||||
| SINSTD96 - unstable deposition rate |
Recipes on PECVD1 for deposition of silicon nitride and silicon oxynitride. Expired!:PECVD1 has been decommissioned
Recipes
| Recipe name | SiH4 flow [sccm] | NH3 flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| 1nitride | 30 | 20 | 1000 | 500 | 80 | |
| 1nit_std | 40 | 20 | 1960 | 550 | 60 | Process control recipe |
Expected results
| Recipe name | Deposition rate [nm/min] | RI | Uniformity [%] | Stress [MPa] | BHF etch rate [Å/min] | Comments |
| 1nitride | ||||||
| 1nit_std | ~32 | 1.89 | ~1 | ~700 | The latest measured values can be seen in the process control sheet in LabManager |