Line 23: Line 23:
[[File:ALD-Sandwich-29a.jpg|700px]]
[[File:ALD-Sandwich-29a.jpg|700px]]


As seen above there is only a very small amount of Ti2p. Why is this? Let us zoom in onto the Ti2p peak and see how the fitting goes.
As seen above there is only a very small amount of Ti2p and at the same time the O1s is much too high. Why is this? Let us zoom in onto the Ti2p peak and see how the fitting goes.


[[File:ALD sandwich Ti survey.gif|630px]]
[[File:ALD sandwich Ti survey.gif|630px]]
Line 30: Line 30:


In the automatic peak fitting routine, a background is added to the data below each peak. This background is then subtracted before the peak is fitted, it is shown with a light green color. It is clear that something goes wrong; the fitted background eats up the majority of the peak. The result is that the fitted Ti2p peak is much too small - then oxygen is seen as the only peak in the spectrum.
In the automatic peak fitting routine, a background is added to the data below each peak. This background is then subtracted before the peak is fitted, it is shown with a light green color. It is clear that something goes wrong; the fitted background eats up the majority of the peak. The result is that the fitted Ti2p peak is much too small - then oxygen is seen as the only peak in the spectrum.
Judging by the way the background is fitted, it looks as if the software is programmed to fit the background below only the Ti2p<sub>3/2</sub> peak. separate peaks of

Revision as of 15:06, 16 October 2018

Survey spectrum processing

This analysis is continued from here.

Under Display options select 'Stacked Chart View' as seen below. One can see that the peaks in the sandwich emerge and disappear as the depth profile progresses.

Pressing the Automatic Survey ID button will therefore only identify the elements present at each individual level. This is shown below for level 33.

We therefore have to add the remaining peaks manually - this is done by pressing the 'ID' button. In the panel below, select the elements from the periodic table, highlight the peak as shown below with Al2p and press 'Add Peaks'.

Once all the peaks have been added to the peak table, one can create a profile as shown below. Among the profile types choose 'Atomic %'.

In the profile below there is one problem.

As seen above there is only a very small amount of Ti2p and at the same time the O1s is much too high. Why is this? Let us zoom in onto the Ti2p peak and see how the fitting goes.

In the gif file above one can see the etch level in the bottom center right.

In the automatic peak fitting routine, a background is added to the data below each peak. This background is then subtracted before the peak is fitted, it is shown with a light green color. It is clear that something goes wrong; the fitted background eats up the majority of the peak. The result is that the fitted Ti2p peak is much too small - then oxygen is seen as the only peak in the spectrum.

Judging by the way the background is fitted, it looks as if the software is programmed to fit the background below only the Ti2p3/2 peak. separate peaks of