Specific Process Knowledge/Etch/III-V ICP/InP-InGaAsP-InGaAs: Difference between revisions
Appearance
| Line 81: | Line 81: | ||
Image:S4_30dg_midt_10.jpg| 30 dg view: low roughness in the trenches | Image:S4_30dg_midt_10.jpg| 30 dg view: low roughness in the trenches | ||
Image:S4_30dg_midt_11.jpg|30 dg view: low roughness in the trenches | Image:S4_30dg_midt_11.jpg|30 dg view: low roughness in the trenches | ||
Image:S4_midt_05.jpg|: | Image:S4_midt_05.jpg|Top view: low roughness in trench and in the large area | ||
</gallery> | </gallery> | ||
Revision as of 13:32, 19 June 2018
Feedback to this page: click here
InP/InGaAsP/InGaAs etch
Unselective etch for large sized features and small aspect ratios by David Larsson, DTU Photonics, 2011
| Recipe | InP Etch 1/InP Precond 1 |
| Cl2 flow | 20 sccm |
| N2 flow | 40 sccm |
| Ar flow | 10 sccm |
| Platen power | 100 W |
| Coil power | 500 W |
| Pressure | 2 mTorr |
| Platen chiller temperature | 180 oC |
| Results (InP Etch 1) | |
| Etch rate | 500-600 nm/min |
| Sidewall angle | 86-87 o |
| Selectivity (InP:SiO2, InP:HSQ) | 50:1 |
- Result of InP etching. David Larsson, DTU Photonics, 2011
InP etching June 2018
Etching of an InP piece on Si carrier
InP piece patterned with SiO2. The piece was etched on top of a Si wafer without bonding. The recipe "InP etch" was used. The roughness looks high in the bottom of the etched areas, especially in the large open areas.
- Result of InP etching.
-
low roughness in narrow trenched
-
low roughness in narrow trenched
-
A little higher roughnedd is larger trences
-
Much larger roughness in open areas
-
Zoom in on the large roughness
-
closed look at the large roughness in the open areas.
Etching of an InP piece on SiO2 carrier
InP piece patterned with SiO2. The piece was etched on top of a Si wafer coated with SiO2 without bonding. The recipe "InP etch" was used. The roughness looks low in the bottom of the etched areas, even in the large open areas.
- Result of InP etching.
-
Top view: oxide is gone on the narrow lines, low roughness in the trenches.
-
Top view: low roughness in the trenches.
-
30 dg view: low roughness in the trenches
-
30 dg view: low roughness in the trenches
-
Top view: low roughness in trench and in the large area