==InP etching June 2018== | ==InP etching June 2018== | ||
===With InP piece on Si carrier=== | ===With InP piece on Si carrier=== | ||
InP piece patterned with SiO2. The pice was etched on | InP piece patterned with SiO2. The pice was etched on top of a Si wafer without bonding. The "InP etch" was used. | ||
<gallery caption="Result of InP etching." widths="500px" heights="400px" perrow="3"> | <gallery caption="Result of InP etching." widths="500px" heights="400px" perrow="3"> | ||
Image:S1_30dg_09.jpg | Image:S1_30dg_09.jpg|low roughness in narrow trenched | ||
Image:S1_30dg_10.jpg | Image:S1_30dg_10.jpg|low roughness in narrow trenched | ||
Image:S1_30dg_midt_14.jpg | Image:S1_30dg_midt_14.jpg|A little higher roughnedd is larger trences | ||
Image:S1_30dg_midt_13.jpg | Image:S1_30dg_midt_13.jpg|Much larger roughness in open areas | ||
Image:S1_30dg_midt_12.jpg | Image:S1_30dg_midt_12.jpg|Zoom in on the large roughness | ||
Image:S1_30dg_midt_11.jpg | Image:S1_30dg_midt_11.jpg|closed look at the large roughness in the open areas. | ||
</gallery> | </gallery> | ||
Revision as of 13:20, 19 June 2018
Feedback to this page: click here
InP/InGaAsP/InGaAs etch
Unselective etch for large sized features and small aspect ratios by David Larsson, DTU Photonics, 2011
| Recipe | InP Etch 1/InP Precond 1 |
| Cl2 flow | 20 sccm |
| N2 flow | 40 sccm |
| Ar flow | 10 sccm |
| Platen power | 100 W |
| Coil power | 500 W |
| Pressure | 2 mTorr |
| Platen chiller temperature | 180 oC |
| Results (InP Etch 1) | |
| Etch rate | 500-600 nm/min |
| Sidewall angle | 86-87 o |
| Selectivity (InP:SiO2, InP:HSQ) | 50:1 |
- Result of InP etching. David Larsson, DTU Photonics, 2011
InP etching June 2018
With InP piece on Si carrier
InP piece patterned with SiO2. The pice was etched on top of a Si wafer without bonding. The "InP etch" was used.
- Result of InP etching.
-
low roughness in narrow trenched
-
low roughness in narrow trenched
-
A little higher roughnedd is larger trences
-
Much larger roughness in open areas
-
Zoom in on the large roughness
-
closed look at the large roughness in the open areas.