Jump to content

Specific Process Knowledge/Lithography/EBeamLithography/High resolution patterning with HSQ: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
Created page with "* ''This work was done by Bingdong Chang and Xiaoli Zhu in 2016;'' * ''This page was edited by Bingdong Chang 23 October 2017.'' High resolution patterns (sub-10nm dots with..."
 
Bghe (talk | contribs)
No edit summary
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/EBeamLithography/High_resolution_patterning_with_HSQ click here]'''
* ''This work was done by Bingdong Chang and Xiaoli Zhu in 2016;''
* ''This work was done by Bingdong Chang and Xiaoli Zhu in 2016;''



Revision as of 14:01, 26 October 2017

Feedback to this page: click here

  • This work was done by Bingdong Chang and Xiaoli Zhu in 2016;
  • This page was edited by Bingdong Chang 23 October 2017.

High resolution patterns (sub-10nm dots with 20nm pitch, sub-10nm lines with 50nm pitch) can be patterned with HSQ resist. Some SEM images are shown as below:

The details of the process is shown below in the table:

It should be noticed that to reduce the broadening of patterns caused by forward and backward scattered electrons, the HSQ resist was first thinned down to below 50nm using BHF before exposure. The etch rate of HSQ with different concentration of BHF is shown as below.

The details of the process is shown below in the table:

The patterns were successfully transferred into silicon by dry etching (with ASE, recipe Pxnano2)

Notice that roughness could be generated during etch by redeposition of HSQ hard mask. For more details, please contact Bingdong Chang (bincha@dtu.dk).