Jump to content

Specific Process Knowledge/Characterization/Profiler/Optical Profiler (Sensofar) acceptance test: Difference between revisions

Bghe (talk | contribs)
Bghe (talk | contribs)
Line 155: Line 155:
| align="center" style="background:#f0f0f0;"|''''''
| align="center" style="background:#f0f0f0;"|''''''
| align="center" style="background:#f0f0f0;"|'''Measured depth [nm]'''
| align="center" style="background:#f0f0f0;"|'''Measured depth [nm]'''
| align="center" style="background:#f0f0f0;"|'''Repeated 20170925 with cover off'''
|-
|-
| 1||337.5
| 1||337.5||347.9
|-
|-
| 2||336.5
| 2||336.5||333.9
|-
|-
| 3||334.7
| 3||334.7||341.5
|-
|-
| 4||335.5
| 4||335.5||343.2
|-
|-
| 5||339.2
| 5||339.2||347.7
|-
|-
| 6||337.2
| 6||337.2||345.4
|-
|-
| 7||334.2
| 7||334.2||341.8
|-
|-
| 8||335.5
| 8||335.5||337.9
|-
|-
| 9||341.1
| 9||341.1||342.1
|-
|-
| 10||344.4
| 10||344.4||335.9
|-
|-
|Average depth||337.58
|Average depth||337.58||341.73
|-
|-
|Repeatability||3% (the bad repeatability was accepted due to the high noise level in the room)