Specific Process Knowledge/Thermal Process/Oxidation: Difference between revisions
| Line 2: | Line 2: | ||
==Oxidation== | ==Oxidation== | ||
At Danchip we have | At Danchip we have seven furnaces for thermal oxidation of silicon samples: Boron Drive-in + Pre-dep furnace (A1), Gate Oxide furnace (A2). Phosphorous Drive-in furnace (A3), Anneal-oxide furnace (C1), Anneal-Bond furnace (C3), Al-Anneal furnace (C3), APOX furnace (D1), Noble furnace and Multipurpose Annealing furnace. | ||
Thermal oxidation can take place either by a dry process or a wet process, depending on what furnace that is used for the oxidation. The film quality for a dry oxide is better than the film quality for a wet oxide with regards to density and dielectric constant. However, the oxidation rate is slow for a dry oxide. | |||
*Dry oxidation is used for 5 nm - 200 nm of oxide and can be grown in the furnaces: A1, A2, A3, C1, C3, Multipurpose Annealing | *Dry oxidation is used for 5 nm - 200 nm of oxide and can be grown in the furnaces: A1, A2, A3, C1, C3, C4, Noble furnace, Multipurpose Annealing | ||
*Wet oxidation is used for up to 4 µm of oxide and can be grown in the furnaces: A1, A3, D1. | *Wet oxidation is used for up to 4 µm of oxide and can be grown in the furnaces: A1, A3, D1. | ||
*Very thick oxide layers >4 µm can be grown in D1 by a wet oxidation (only performed by Danchip). | *Very thick oxide layers >4 µm can be grown in D1 by a wet oxidation (only performed by Danchip). | ||
Revision as of 11:10, 30 August 2017
Feedback to this page: click here
Oxidation
At Danchip we have seven furnaces for thermal oxidation of silicon samples: Boron Drive-in + Pre-dep furnace (A1), Gate Oxide furnace (A2). Phosphorous Drive-in furnace (A3), Anneal-oxide furnace (C1), Anneal-Bond furnace (C3), Al-Anneal furnace (C3), APOX furnace (D1), Noble furnace and Multipurpose Annealing furnace.
Thermal oxidation can take place either by a dry process or a wet process, depending on what furnace that is used for the oxidation. The film quality for a dry oxide is better than the film quality for a wet oxide with regards to density and dielectric constant. However, the oxidation rate is slow for a dry oxide.
- Dry oxidation is used for 5 nm - 200 nm of oxide and can be grown in the furnaces: A1, A2, A3, C1, C3, C4, Noble furnace, Multipurpose Annealing
- Wet oxidation is used for up to 4 µm of oxide and can be grown in the furnaces: A1, A3, D1.
- Very thick oxide layers >4 µm can be grown in D1 by a wet oxidation (only performed by Danchip).
The standard recipes, quality control limits and results for the Boron Drive-in + Pre-dep furnace (A1) and the Phosphorus Drive-in furnace (A3) can be found here:
- Standard recipes, QC limits and results for the Boron Drive-in + Predep furnace (A1)
- Standard recipes, QC limits and results for the Phosphorus Drive-in furnace (A3)
The wet oxidation rates for the Anneal-Bond furnace (C1) can be found here:
Comparison of the seven oxidation furnaces
| Generel description | Dry and wet oxidation. Boron pre-deposition and boron drive-in of boron are also done in the furnace. | Dry oxidation of gate oxide and other very clean oxides. | Dry and wet oxidation. Phosphorous drive-in is also done in the furnace. | Dry and wet oxidation of 100 mm and 150 mm wafers. Oxidation of new wafers without RCA cleaning. Oxidation and annealing of wafers from the LPCVD furnaces and PECVD4. | Dry and wet oxidation and annealing of wafers from Wafer Bonder 02 and from PECVD4 and PECVD3. | Wet oxidation of very thick oxides > 4 µm. | Dry oxidation and annealing of almost all materials. |
|---|---|---|---|---|---|---|---|
| Oxidation method |
|
|
|
|
|
|
|
| Annealing gas |
|
|
|
|
|
|
|
| Process temperature |
|
|
|
|
|
|
|
| Substrate and batch size |
|
|
|
|
|
|
|
| Allowed materials |
|
|
|
|
|
|
|
Oxidation curves
Color chart for oxide/nitride thickness
Generic calculator for wet/dry oxide thickness calculation
The following links give an approximate oxide time/thickness based on a general formula:
Deal-Grove parameters
By Kasper Reck-Nielsen February 2015
The following table contains linear and parabolic parameters for use in the Deal-Grove model for thermal oxidation. The parameters are obtained a least squares fit to data available in the furnace logbooks. Information on wafer orientation and doping concentration, which is not available in the logbooks, has not been included in calculating the parameters.
| Anneal Oxide | Anneal Bond | Boron Drive-in | Gate Oxide | Phosphor Drive-in | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Recipe | B [µm2/h] | B/A [µm/h] | RMSE [nm] | B [µm2/h] | B/A [µm/h] | RMSE [nm] | B [µm2/h] | B/A [µm/h] | RMSE [nm] | B [µm2/h] | B/A [µm/h] | RMSE [nm] | B [µm2/h] | B/A [µm/h] | RMSE [nm] |
| DRY900 | 0.000408 | 0.107 | Too little data | 0.0660 | 0.272 | 31 | 0.000390 | 0.154 | Too little data | 0.0028 | 0.079 | 4 (limited data) | 0.0507 | 0.884 | Too little data |
| DRY1000 | - | - | - | - | - | - | 0.465 | 0.838 | 20 | - | - | - | 0.641 | 1.45 | 41 |
| DRY1050 | 0.0111 | 0.526 | 27 | - | - | - | 0.0129 | 0.330 | 8 | 0.022 | 0.505 | 3 (limited data) | 0.0134 | 0.362 | 6 |
| DRY1100 | 0.020 | 0.930 | 10 | - | - | - | 0.0212 | 0.736 | 23 | - | - | - | 0.0313 | 0.553 | 14 |
| WET950 | - | - | - | - | - | 0.0716 | 1.25 | 12 | - | - | - | 0.110 | 1.17 | 11 | |
| WET1000 | 0.192 | 1.54 | 44 | - | - | 0.192 | 1.80 | 29 | - | - | - | 0.195 | 2.49 | 22 | |
| WET1050 | 0.487 | 0.965 | 29 | 0.477 | 0.899 | Too little data | 0.455 | 1.33 | 16 | - | - | - | 0.448 | 1.73 | 12 |
| WET1100 | 0.580 | 1.43 | 8 | - | - | - | 0.519 | 1.186 | 3 | - | - | - | 0.403 | 9.05 | 7 |
Wet Oxidation on <100>
The curves below are based on measurements in our specific furnaces and give more accurate results. We will still recommend to make minimum one test run if the thickness is very important.
- Wet oxidation
-
A1 Furnace <100>-Si Wet Oxidation
-
A3 Furnace <100>-Si Wet Oxidation
Dry Oxidation on <100> and <111> wafer
- Dry oxidation
-
Dry oxide on <100> wafer. The y-axis is in Å and the x-axis is in minutes.
-
Dry oxide on <111> wafer. The y-axis is in Å and the x-axis is in minutes.