Specific Process Knowledge/Etch/ICP Metal Etcher/silicon oxide/By BGHE: Difference between revisions
| Line 5: | Line 5: | ||
I started out with a recipe developed by Peixiong called pxSiO2try9, look at his results [[Specific Process Knowledge/Etch/ICP Metal Etcher/silicon oxide/By Peixiong| here]] | I started out with a recipe developed by Peixiong called pxSiO2try9, look at his results [[Specific Process Knowledge/Etch/ICP Metal Etcher/silicon oxide/By Peixiong| here]] | ||
{| border="1" cellspacing="1" cellpadding="1" align="left" | {|style="width:1500px" border="1" cellspacing="1" cellpadding="1" align="left" | ||
! Parameter | ! Parameter | ||
! '''Mask material''' | ! '''Mask material''' | ||
| Line 17: | Line 17: | ||
! width="20"| '''T''' | ! width="20"| '''T''' | ||
! '''Process time''' | ! '''Process time''' | ||
! width=" | ! width="200"| '''Comment''' | ||
! width=" | ! width="200"|'''Results''' | ||
! width=" | ! width="200"|'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | ||
trench opening as a fraction of pitch | trench opening as a fraction of pitch | ||
! '''Profile angles''' | ! '''Profile angles''' | ||
| Line 41: | Line 41: | ||
|<!--'''T'''--> 0 | |<!--'''T'''--> 0 | ||
|<!--'''Process time'''--> 1:30min | |<!--'''Process time'''--> 1:30min | ||
|width=" | |width="200"|<!--'''Comment'''--> The layer in this case is 300nm Si3N4 | ||
|width=" | |width="200"|<!--'''Results'''--> | ||
[[File:s008684_Si3N4_19.jpg|100px|frameless]] [[File:s008684_Si3N4_20.jpg|100px|frameless]] | [[File:s008684_Si3N4_19.jpg|100px|frameless]] [[File:s008684_Si3N4_20.jpg|100px|frameless]] | ||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | ||
| Line 73: | Line 73: | ||
|<!--'''T'''--> 0 | |<!--'''T'''--> 0 | ||
|<!--'''Process time'''--> 10min | |<!--'''Process time'''--> 10min | ||
|width=" | |width="200"|<!--'''Comment'''--> | ||
|width=" | |width="200"|<!--'''Results'''--> | ||
[[File:ICP metal s007467_07.jpg|100px|frameless]] [[File:ICP metal s007467_09.jpg|100px|frameless]] | [[File:ICP metal s007467_07.jpg|100px|frameless]] [[File:ICP metal s007467_09.jpg|100px|frameless]] | ||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | ||
| Line 110: | Line 110: | ||
|<!--'''T'''--> 0 | |<!--'''T'''--> 0 | ||
|<!--'''Process time'''--> 5min | |<!--'''Process time'''--> 5min | ||
|width=" | |width="200"|<!--'''Comment'''--> | ||
|width=" | |width="200"|<!--'''Results'''--> | ||
[[File:ICP metal s007418_09.jpg|100px|frameless]] [[File:ICP metal s007418_12.jpg|100px|frameless]] | [[File:ICP metal s007418_09.jpg|100px|frameless]] [[File:ICP metal s007418_12.jpg|100px|frameless]] | ||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | ||
| Line 143: | Line 143: | ||
|<!--'''T'''--> 0 | |<!--'''T'''--> 0 | ||
|<!--'''Process time'''--> 8min | |<!--'''Process time'''--> 8min | ||
|width=" | |width="200"|<!--'''Comment'''--> repeated s007416 and s007468 with a barc etch step. This improved the uniformity of the etch performance over different linewidth and improved the selectivity to the mask and the profile angle. After this I continued with barc etch. '''Nice''' | ||
|width=" | |width="200"|<!--'''Results'''--> | ||
[[File:ICP metal s007565_02.jpg|100px|frameless]] [[File:ICP metal s007565_06.jpg|100px|frameless]] | [[File:ICP metal s007565_02.jpg|100px|frameless]] [[File:ICP metal s007565_06.jpg|100px|frameless]] | ||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | ||
| Line 181: | Line 181: | ||
|<!--'''T'''--> 0 | |<!--'''T'''--> 0 | ||
|<!--'''Process time'''--> 10min | |<!--'''Process time'''--> 10min | ||
|width=" | |width="200"|<!--'''Comment'''--> Repeated s007416 with double time. | ||
|width=" | |width="200"|<!--'''Results'''--> | ||
[[File:ICP metal s007468_12.jpg|100px|frameless]] [[File:ICP metal s007468_15.jpg|100px|frameless]] | [[File:ICP metal s007468_12.jpg|100px|frameless]] [[File:ICP metal s007468_15.jpg|100px|frameless]] | ||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | ||
| Line 223: | Line 223: | ||
|<!--'''T'''--> 0 | |<!--'''T'''--> 0 | ||
|<!--'''Process time'''--> 5min | |<!--'''Process time'''--> 5min | ||
|width=" | |width="200"|<!--'''Comment'''--> From S007411 the platen power was decreased to avoid trenching. The etch rate went down and some variation in profile angle is seen from small opening to large opening. Started plasma on the 4th try | ||
|width=" | |width="200"|<!--'''Results'''--> | ||
[[File:ICP metal s007416_05.jpg|100px|frameless]] [[File:ICP metal s007416_06.jpg|100px|frameless]] | [[File:ICP metal s007416_05.jpg|100px|frameless]] [[File:ICP metal s007416_06.jpg|100px|frameless]] | ||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | ||
| Line 260: | Line 260: | ||
|<!--'''T'''--> 0 | |<!--'''T'''--> 0 | ||
|<!--'''Process time'''--> 5min | |<!--'''Process time'''--> 5min | ||
|width=" | |width="200"|<!--'''Comment'''--> From s007409 the Gas flow ratio between C4F8 and H2 has been changed to more C4F8 and less H2. This increased the etch rate (more fluorine). Trenching is seen and tappered sidewall is seen indicating a more physical etch. | ||
|width=" | |width="200"|<!--'''Results'''--> | ||
[[File:ICP metal s007411_01.jpg|100px|frameless]] [[File:ICP metal s007411_02.jpg|100px|frameless]] | [[File:ICP metal s007411_01.jpg|100px|frameless]] [[File:ICP metal s007411_02.jpg|100px|frameless]] | ||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | ||
| Line 291: | Line 291: | ||
|<!--'''T'''--> 0 | |<!--'''T'''--> 0 | ||
|<!--'''Process time'''--> 5min | |<!--'''Process time'''--> 5min | ||
|width=" | |width="200"|<!--'''Comment'''--> Increased the platen power. The selectivity and profile looks good but the resist profile has been rounded more on the edge and this will effect the profile for a deeper etch. | ||
|width=" | |width="200"|<!--'''Results'''--> | ||
[[File:ICP metal s007419_17.jpg|100px|frameless]] [[File:ICP metal s007419_21.jpg|100px|frameless]] | [[File:ICP metal s007419_17.jpg|100px|frameless]] [[File:ICP metal s007419_21.jpg|100px|frameless]] | ||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | ||
| Line 325: | Line 325: | ||
|<!--'''T'''--> 0 | |<!--'''T'''--> 0 | ||
|<!--'''Process time'''--> 7min | |<!--'''Process time'''--> 7min | ||
|width=" | |width="200"|<!--'''Comment'''--> Reduced the platen power.Effect: ARDE - less CD increase but more possitive tappered profile. | ||
|width=" | |width="200"|<!--'''Results'''--> | ||
[[File:ICP metal s007410_05.jpg|100px|frameless]] [[File:ICP metal s007410_09.jpg|100px|frameless]] | [[File:ICP metal s007410_05.jpg|100px|frameless]] [[File:ICP metal s007410_09.jpg|100px|frameless]] | ||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | ||
| Line 359: | Line 359: | ||
|<!--'''T'''--> 0 | |<!--'''T'''--> 0 | ||
|<!--'''Process time'''--> 10min | |<!--'''Process time'''--> 10min | ||
|width=" | |width="200"|<!--'''Comment'''--> Tried with C4F8/Ar instead of C4F8/H2 => much lower etch rate and bad selectivity to the resist. | ||
|width=" | |width="200"|<!--'''Results'''--> | ||
[[File:ICP metal s006656 no1.jpg|100px|frameless]] [[File:ICP metal s006656 no2.jpg|100px|frameless]] | [[File:ICP metal s006656 no1.jpg|100px|frameless]] [[File:ICP metal s006656 no2.jpg|100px|frameless]] | ||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | ||
| Line 390: | Line 390: | ||
|<!--'''T'''--> 0 | |<!--'''T'''--> 0 | ||
|<!--'''Process time'''--> 5min | |<!--'''Process time'''--> 5min | ||
|width=" | |width="200"|<!--'''Comment'''--> Repeated Pexiongs recipe without barc etch and only 5 min's runs. It probably takes about 1 min to get through the barc. If you count that in then the etch rate and relectivity to resist is almost the same as for the first run. Effect: CD increase | ||
|width=" | |width="200"|<!--'''Results'''--> | ||
[[File:ICP metal s007409_06.jpg|100px|frameless]] [[File:ICP metal s007409_07.jpg|100px|frameless]] | [[File:ICP metal s007409_06.jpg|100px|frameless]] [[File:ICP metal s007409_07.jpg|100px|frameless]] | ||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | ||
| Line 425: | Line 425: | ||
|<!--'''T'''--> 0 | |<!--'''T'''--> 0 | ||
|<!--'''Process time'''--> 10min | |<!--'''Process time'''--> 10min | ||
|width=" | |width="200"|<!--'''Comment'''--> From Peixiong | ||
|width=" | |width="200"|<!--'''Results'''--> | ||
[[File:S0061066_n02.jpg|100px|frameless]] [[File:S006106_n04.jpg|100px|frameless]] | [[File:S0061066_n02.jpg|100px|frameless]] [[File:S006106_n04.jpg|100px|frameless]] | ||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | ||
Revision as of 11:01, 16 June 2017
I tried with two different gas regimes: CF4 and C4F8. I only made a few tests with CF4 since I got a very bad selectivity to the resist mask and I dicided to go for the C4F8 instead.
Zhibo Li @ Danchip has also tried (December 2016) with similar setting, see his results in this file: File:Zhibo Li SiO2 ICP etch (dose205).docx
C4F8 
I started out with a recipe developed by Peixiong called pxSiO2try9, look at his results here
| Parameter | Mask material | Barc etch | Coil power | Platen power | Pressure | Flow rate C4F8 | Flow rate H2 | Flow rate Ar | T | Process time | Comment | Results | CD change (mask 55% trench) after s007467 is it <50% after barc etch trench opening as a fraction of pitch |
Profile angles | Etch depth in SiO2 | Etch rate | Etch depth in resist | Selectivity (resist:SiO2) | Etch rate in Si |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| s008684 | 880nm KRF | barc etch CF 50s | 1000W | 200W | 2.5mTorr | 13sccm | 30sccm | 0 | 0 | 1:30min | The layer in this case is 300nm Si3N4 |
35% (1µm pitch) |
83-88 |
>300nm/min (Si3N4) |
240nm |
~1:2 (Si3N4) |
? | ||
| s007467 (as 18) | 750nm KRF | none | 1000W | 150W | 2.5mTorr | 8sccm | 30sccm | 0 | 0 | 10min |
? (2µm pitch) |
77 (6µm p) |
1015 nm (2µm pitch) |
101.5 nm/min (2µm pitch) |
210nm |
1:4.8 (2µm pitch) |
|||
| s007418 | 750nm KRF | none | 1000W | 150W | 2.5mTorr | 8sccm | 30sccm | 0 | 0 | 5min |
46.5% (2µm pitch) |
87-88 (large structures) |
400 nm (6µm pitch) |
80 nm/min (6µm pitch) |
200nm/76nm? |
1:2 (6µm pitch) |
| ||
| s007565 (as 16) | 880nm KRF | barc etch CF 40s | 800W | 100W | 2.5mTorr | 13sccm | 26sccm | 0 | 0 | 8min | repeated s007416 and s007468 with a barc etch step. This improved the uniformity of the etch performance over different linewidth and improved the selectivity to the mask and the profile angle. After this I continued with barc etch. Nice |
44.5% (2µm pitch) |
87-88 |
779 nm (2µm pitch) |
97.4 nm/min (2µm pitch) |
130nm |
1:6.0 (2µm pitch) |
||
| s007468 (as 16) | 750nm KRF | none | 800W | 100W | 2.5mTorr | 13sccm | 26sccm | 0 | 0 | 10min | Repeated s007416 with double time. |
17.3% (1µm pitch) |
76-78 |
850 nm (1µm pitch) |
85 nm/min (1µm pitch) |
300nm |
1:2.8 (1µm pitch) |
||
| s007416 | 750nm KRF | none | 800W | 100W | 2.5mTorr | 13sccm | 26sccm | 0 | 0 | 5min | From S007411 the platen power was decreased to avoid trenching. The etch rate went down and some variation in profile angle is seen from small opening to large opening. Started plasma on the 4th try |
38.6% (2µm pitch) |
77 (small structures) 90 (large structures) |
346 nm (1.5µm pitch) |
69 nm/min (1.5µm pitch) |
50nm |
1:7 (1.5µm pitch) |
| |
| s007411 | 750nm KRF | none | 800W | 150W | 2.5mTorr | 13sccm | 26sccm | 0 | 0 | 5min | From s007409 the Gas flow ratio between C4F8 and H2 has been changed to more C4F8 and less H2. This increased the etch rate (more fluorine). Trenching is seen and tappered sidewall is seen indicating a more physical etch. |
47.0% (1µm pitch) |
83 |
708 nm |
142 nm/min |
294 nm |
1:2.4 |
||
| s007419 | 750nm KRF | none | 800W | 200W | 2.5mTorr | 8sccm | 30sccm | 0 | 0 | 5min | Increased the platen power. The selectivity and profile looks good but the resist profile has been rounded more on the edge and this will effect the profile for a deeper etch. |
46.6% (1µm pitch) |
86-90 |
270nm (1µm pitch) |
54 nm/min (1µm pitch) |
100nm |
1:4 (2.5µm pitch) |
||
| s007410 | 750nm KRF | none | 800W | 75W | 2.5mTorr | 8sccm | 30sccm | 0 | 0 | 7min | Reduced the platen power.Effect: ARDE - less CD increase but more possitive tappered profile. |
42.3% (2µm pitch) |
80-82 |
0 nm (1µm pitch) |
0 nm/min (1µm pitch) |
100nm |
1:0 (1µm pitch) |
||
| s006656 | 750nm KRF | none | 1000W | 150W | 2.5mTorr | 15sccm | 0sccm | 30sccm | 0 | 10min | Tried with C4F8/Ar instead of C4F8/H2 => much lower etch rate and bad selectivity to the resist. |
358 nm |
35.8 nm/min (2µm pitch) |
526nm |
1:0:68 |
||||
| s007409 | 750nm KRF | none | 800W | 150W | 2.5mTorr | 8sccm | 30sccm | 0 | 0 | 5min | Repeated Pexiongs recipe without barc etch and only 5 min's runs. It probably takes about 1 min to get through the barc. If you count that in then the etch rate and relectivity to resist is almost the same as for the first run. Effect: CD increase |
47.4% (1µm pitch) |
86-89 |
280 nm (1µm pitch) |
56 nm/min (1µm pitch) |
160nm |
1:1.8 (1µm pitch) |
||
| s006106 | 750nm KRF | Barc etch O2 75s | 800W | 150W | 2.5mTorr | 8sccm | 30sccm | 0 | 0 | 10min | From Peixiong |
60% |
79 |
1053 nm (center) |
105 nm/min |
280nm |
1:3:75 (2µm pitch) |
CF4
I stopped trying with CF4 because I got bad selectivty to the resist and decided to focus on the recipe with C4F8 instead.