Revision as of 17:17, 2 April 2008
The Molecular Vapor Deposition Tool

The Applied Microstructures MVD 100 system deposits molecular films on surfaces. These films serve a wide range of purposes ranging from antistiction coatings of nanoimprint lithography stamps to protecting MEMS structures. They are created as self-assembled monolayers on a surface when a molecular vapor of chemials is present. In most cases the chlorine atoms in the end of an flourinated organosilane react with -OH groups of the surface to form a chemical bond under elimination of HCL.
| Common parameters | Multiplexed parameters | |||
|---|---|---|---|---|
| Parameter | Setting | Parameter | Etch | Passivation |
| Temperature | 10oC | SF6 Flow | 260 sccm | 0 sccm |
| No. of cycles | 31 | O2 Flow | 26 sccm | 0 sccm |
| Process time | 5:56 mins | C4F4 Flow | 0 sccm | 120 sccm |
| APC mode | manual | RF coil | 2800 W | 1000 W |
| APC setting | 86.8 % | RF Platen | 16 W | 0 W |
| Cycle time | 6.5 s | 5 s | ||
| Common parameters | Multiplexed parameters | |||
|---|---|---|---|---|
| Parameter | Setting | Parameter | Etch | Passivation |
| Temperature | 10oC | SF6 Flow | 260 sccm | 0 sccm |
| No. of cycles | 31 | O2 Flow | 26 sccm | 0 sccm |
| Process time | 5:56 mins | C4F4 Flow | 0 sccm | 120 sccm |
| APC mode | manual | RF coil | 2800 W | 1000 W |
| APC setting | 86.8 % | RF Platen | 16 W | 0 W |
| Cycle time | 6.5 s | 5 s |