Specific Process Knowledge/Etch/ICP Metal Etcher/silicon oxide/By BGHE: Difference between revisions
| Line 61: | Line 61: | ||
? | ? | ||
|- | |- | ||
|- | |||
|s007411 | |||
|<!-- '''Mask material''' --> 750nm KRF | |||
|<!-- '''Barc etch''' --> none | |||
|<!-- '''Coil power''' --> 800W | |||
|<!--'''Platen power'''--> 150W | |||
|<!--'''Pressure'''--> 2.5mTorr | |||
|<!--'''Flow rate C4F8'''--> 13sccm | |||
|<!--'''Flow rate H2'''--> 26sccm | |||
|<!--'''Flow rate Ar'''-->0 | |||
|<!--'''T'''--> 0 | |||
|<!--'''Process time'''--> 5min | |||
|<!--'''Comment'''--> Increased the platen power. The selectivity and profile looks good but the resist profile has been rounded more on the edge and this will effect the profile for a deeper etch. | |||
|<!--'''Results'''--> | |||
[[File:ICP metal s007419_17.jpg|100px|frameless]] [[File:ICP metal s007419_21.jpg|100px|frameless]] | |||
|<!--'''CD change (mask 55% trench) after s007467 is it <50% after barc etch'''<br> | |||
trench opening as a fraction of pitch--> | |||
47.0% (1µm pitch)<br> | |||
44.6% (2µm pitch)<br> | |||
|<!--'''Profile angles'''--> | |||
83 | |||
|<!--'''Etch depth in SiO2'''--> | |||
708 nm<br> | |||
|<!--'''Etch rate'''--> | |||
142 nm/min | |||
|<!--'''Etch depth in resist'''--> | |||
294 nm | |||
|<!--'''Selectivity (resist:SiO2)'''--> | |||
1:2.4 <br> | |||
|<!--'''Etch rate in Si'''--> | |||
|- | |- | ||
|s007419 | |s007419 | ||
Revision as of 16:51, 16 January 2017
I tried with two different gas regimes: CF4 and C4F8. I only made a few tests with CF4 since I got a very bad selectivity to the resist mask and I dicided to go for the C4F8 instead.
Zhibo Li @ Danchip has also tried (December 2016) with similar setting, see his results in this file: File:Zhibo Li SiO2 ICP etch (dose205).docx
C4F8 
I started out with a recipe developed by Peixiong called pxSiO2try9, look at his results here
| Parameter | Mask material | Barc etch | Coil power | Platen power | Pressure | Flow rate C4F8 | Flow rate H2 | Flow rate Ar | T | Process time | Comment | Results | CD change (mask 55% trench) after s007467 is it <50% after barc etch trench opening as a fraction of pitch |
Profile angles | Etch depth in SiO2 | Etch rate | Etch depth in resist | Selectivity (resist:SiO2) | Etch rate in Si |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| s008684 | 880nm KRF | barc etch CF 50s | 1000W | 200W | 2.5mTorr | 13sccm | 30sccm | 0 | 0 | 1:30min | The layer in this case is 300nm Si3N4 |
35% (1µm pitch) |
83-88 |
>300nm/min (Si3N4) |
240nm |
~1:2 (Si3N4) |
? | ||
| s007411 | 750nm KRF | none | 800W | 150W | 2.5mTorr | 13sccm | 26sccm | 0 | 0 | 5min | Increased the platen power. The selectivity and profile looks good but the resist profile has been rounded more on the edge and this will effect the profile for a deeper etch. |
47.0% (1µm pitch) |
83 |
708 nm |
142 nm/min |
294 nm |
1:2.4 |
||
| s007419 | 750nm KRF | none | 800W | 200W | 2.5mTorr | 8sccm | 30sccm | 0 | 0 | 5min | Increased the platen power. The selectivity and profile looks good but the resist profile has been rounded more on the edge and this will effect the profile for a deeper etch. |
46.6% (1µm pitch) |
86-90 |
270nm (1µm pitch) |
54 nm/min (1µm pitch) |
100nm |
1:4 (2.5µm pitch) |
||
| s007410 | 750nm KRF | none | 800W | 75W | 2.5mTorr | 8sccm | 30sccm | 0 | 0 | 7min | Reduced the platen power.Effect: ARDE - less CD increase but more possitive tappered profile. |
42.3% (2µm pitch) |
80-82 |
0 nm (1µm pitch) |
0 nm/min (1µm pitch) |
100nm |
1:0 (1µm pitch) |
||
| s006656 | 750nm KRF | none | 1000W | 150W | 2.5mTorr | 15sccm | 0sccm | 30sccm | 0 | 10min | Tried with C4F8/Ar instead of C4F8/H2 => much lower etch rate and bad selectivity to the resist. |
358 nm |
35.8 nm/min (2µm pitch) |
526nm |
1:0:68 |
||||
| s007409 | 750nm KRF | none | 800W | 150W | 2.5mTorr | 8sccm | 30sccm | 0 | 0 | 5min | Repeated Pexiongs recipe without barc etch and only 5 min's runs. It probably takes about 1 min to get through the barc. If you count that in then the etch rate and relectivity to resist is almost the same as for the first run. Effect: CD increase |
47.4% (1µm pitch) |
86-89 |
280 nm (1µm pitch) |
56 nm/min (1µm pitch) |
160nm |
1:1.8 (1µm pitch) |
||
| s006106 | 750nm KRF | Barc etch O2 75s | 800W | 150W | 2.5mTorr | 8sccm | 30sccm | 0 | 0 | 10min | From Peixiong |
60% |
79 |
1053 nm (center) |
105 nm/min |
280nm |
1:3:75 (2µm pitch) |
CF4
I stopped trying with CF4 because I got bad selectivty to the resist and decided to focus on the recipe with C4F8 instead.