Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Gold: Difference between revisions

From LabAdviser
Paphol (talk | contribs)
Pevo (talk | contribs)
Line 19: Line 19:
! Sputter coater [[Specific Process Knowledge/Thin film deposition/Sputter coater#The_Hummer_Sputter_coater|Hummer]]   
! Sputter coater [[Specific Process Knowledge/Thin film deposition/Sputter coater#The_Hummer_Sputter_coater|Hummer]]   
! Sputter coater [[Specific Process Knowledge/Thin film deposition/Sputter coater#The_Balzer_Sputter_coater|Balzer]]
! Sputter coater [[Specific Process Knowledge/Thin film deposition/Sputter coater#The_Balzer_Sputter_coater|Balzer]]
! Sputter coater [[Specific Process Knowledge/Thin film deposition/Sputter coater#The_Balzer_Sputter_coater|Sputter coater 03]]
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
! General description
! General description
Line 25: Line 26:
| Sputter deposition of Au
| Sputter deposition of Au
| E-beam deposition of Au
| E-beam deposition of Au
| Sputter deposition of Au
| Sputter deposition of Au
| Sputter deposition of Au
| Sputter deposition of Au
| Sputter deposition of Au
Line 37: Line 39:
|
|
|
|
 
|
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
! Layer thickness
! Layer thickness
Line 46: Line 48:
|
|
|
|
 
|Not measured
|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
Line 56: Line 58:
|Not measured
|Not measured
|Not measured
|Not measured
 
|Not measured
|-
|-


Line 82: Line 84:
*1 large sample (< 4" wafer)
*1 large sample (< 4" wafer)
*Several smaller samples
*Several smaller samples
 
|
*1x4" wafer
*Several smaller samples
|-
|-


Line 120: Line 124:
* Quartz wafers  
* Quartz wafers  
* Pyrex wafers
* Pyrex wafers
|
|
|
* All samples allowed in the SEM Supra 1
|.
|.
|.
|.
Line 135: Line 143:
|
|


|Used to gold sputter coating of   
|Used for gold sputter coating of   
samples mainly before SEM characterization
samples before SEM inspection
|Used to gold sputter coating of  
|Used for gold sputter coating of  
samples mainly before SEM characterization
samples before SEM inspection
 
|Used for gold sputter coating of
samples before SEM inspection
|-
|-
|}
|}

Revision as of 11:17, 26 September 2016

4th Level - Comparison

Feedback to this page: click here

Gold can be deposited by e-beam evaporation or sputtering. In the chart below you can compare the different deposition equipment.


Adhesion of Au on Si

The adhesion of gold on Silicon or Silicon with native oxide is not very good. The Si substrate is often deposited an adhesion layer before the gold deposition. A few nm of Chromium or Titanium works well and they react with the Oxygen of Silicon oxide and present a metallic bond with gold. 5 nm to 10 nm thick of Cr or Ti is commonly used and it is important to deposit Cr or Ti and then immediately Au. If the vacuum chamber is opened in between, the surface of Cr or Ti will get oxidized and that will give a poor adhesion. If a gold layer needs to be deposited directly on Silicon, then native oxide has to be removed by deep in diluted HF and immediately load the evaporation chamber. And after the deposition, the wafer has to be heated op to get some Au-Si diffusion which improves the adhesion.


E-beam evaporation (Alcatel) E-beam evaporation (Wordentec) Sputter (Lesker) E-beam evaporation (Physimeca) Sputter coater Hummer Sputter coater Balzer Sputter coater Sputter coater 03
General description E-beam deposition of Au E-beam deposition of Au Sputter deposition of Au E-beam deposition of Au Sputter deposition of Au Sputter deposition of Au Sputter deposition of Au
Pre-clean RF Ar clean RF Ar clean RF Ar clean
Layer thickness 10 Å to 5000Å* 10 Å to 5000Å* 10 Å to 10Å to about 3000Å* Not measured
Deposition rate 2 Å/s to 10 Å/s 1 Å/s to 10 Å/s From 5 Å/s up to 10Å/s Not measured Not measured Not measured
Batch size
  • Up to 1x4" wafers
  • smaller pieces
  • 24x2" wafers or
  • 6x4" wafers or
  • 6x6" wafers
  • Pieces or
  • 1x4" wafer or
  • 1x6" wafer
  • 1x 2" wafer or
  • 1x 4" wafers or
  • Several smaller pieces
  • 1x4" wafer
  • Several smaller samples
  • 1 large sample (< 4" wafer)
  • Several smaller samples
  • 1x4" wafer
  • Several smaller samples
Allowed materials
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Silicon
  • Silicon oxide
  • Silicon nitride
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Carbon
  • III-V materials
  • Silicon wafers
  • Quartz wafers
  • Pyrex wafers
  • All samples allowed in the SEM Supra 1
. .


Comment
  • For thicknesses above 200 nm permission is required
  • An adhesion layer (of Cr or Ti) is recommended under Au.
  • For thicknesses above 200 nm permission is required
  • An adhesion layer (of Cr or Ti) is recommended under Au.
Used for gold sputter coating of

samples before SEM inspection

Used for gold sputter coating of

samples before SEM inspection

Used for gold sputter coating of

samples before SEM inspection


* For thicknesses above 200 nm permission from ThinFilm group (thinfilm@danchip.dtu.dk) is required.

Studies of Au deposition processes in the Wordentec

Roughness of Au layers - Roughness of Au layers deposited with different equipment and settings

Wafer temperature

The wafer temperature during e-beam deposition of 200 nm Au on six wafers has been measured using thermal labels on the backside of the wafers. The following results were obtained:

Wafer Temperature [C]
1 48
2 60
3 65
4 71
5 71
6 77

The temperatures are accurate within approximately +/- 3C and probably underestimating the actual wafer temperature slightly. It is observed that the wafer temperature increases with each wafer, thus if wafer temperature is of concern it is advised to reduce the number of wafers per run.