== 3 week project on mrEBL6000 by William Tiddi == | == 3 week project on mrEBL6000 by William Tiddi == | ||
mrEBL6000 was studied April 2015 by William Tiddi; the report can be found [[:File:Report (2).pdf here]] | mrEBL6000 was studied April 2015 by William Tiddi; the report can be found [[:File:Report (2).pdf here]] | ||
<br> | |||
<br> | |||
<br> | |||
== Spin Curve == | == Spin Curve == | ||
Revision as of 10:53, 6 July 2016
| Resist | Polarity | Manufacturer | Comments | Technical reports | Developer | Rinse | Remover | Process flows (in docx-format) |
| mr EBL 6000.1 | Positive | MicroResist | Standard negative resist | mrEBL6000 processing Guidelines.pdf | mr DEV | IPA | mr REM | Process_Flow_mrEBL6000.docx |
3 week project on mrEBL6000 by William Tiddi
mrEBL6000 was studied April 2015 by William Tiddi; the report can be found File:Report (2).pdf here
Spin Curve

The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only.
9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.
| MicroResist mr EBL 6000. Spin coated on Spin Coater: Manual LabSpin A-5, WILTID, 2015. Softbake 3 min @ 110 degC. | ||
|---|---|---|
| Spin Speed [rpm] | Thickness [nm] | St Dev |
| 2000 | 103 | 0.5 |
| 3000 | 88 | 0.4 |
| 4000 | 78 | 0.4 |
| 5000 | 71 | 0.7 |
| 6000 | 68 | 0.5 |
| 7000 | 66 | 0.6 |
| MicroResist mr EBL 6000 diluted 1:1 in anisole. Spin coated on Spin Coater: Manual LabSpin A-5, WILTID, 2015. Softbake 3 min @ 110 degC. | ||
|---|---|---|
| Spin Speed [rpm] | Thickness [nm] | St Dev |
| 2000 | 50 | 0.2 |
| 3000 | 42 | 0.5 |
| 4000 | 38 | 0.5 |
| 5000 | 34 | 0.3 |
| 6000 | 32 | 0.3 |
| 7000 | 32 | 0.3 |