* Bake-out at 250 C (>2,5 hours)
* Bake-out at 250 C (>2,5 hours)
* Plasma ashing
* Plasma ashing
* Sputter-deposit in Alcatel: Power: 550W, Ar-pressure: 10<math>^{-2}</math> mbar (base pressure: 10<math>^{-6}</math> mbar   
* Sputter-deposit in Alcatel: Power: 550W, Ar-pressure: 10<math>^{-2}</math> mbar (base pressure: 10<math>^{-6}</math> mbar)
* Patterning of the silicon using either wet (poly-etch) or dry etching
   


40% HF 3µm/min
40% HF 3µm/min

Revision as of 12:36, 11 March 2008

At Danchip, we have two types of bulk glass substrates: Borosilicate glass (Borofloat 33 (like pyrex)) and fused silicate glass which in cleanliness is similar to quartz. Both types are etched wet in a special set-up placed in a fumehood using a strong HF-solution (isotropic etch). The set-up consists of a 5 l plasic beaker placed on a stirring plate (magnetic stirring) and a special horizontal wafer holder. Normally a 40% pre-mixed HF solution is used.

Masking materials and pre-treatment of the glass surface prior to the deposition of the masking material is a special concern in particular for deep etchings (> 10µm).

Due to the high cleanliness fused silica is allowed access to basically all machines meaning that e.g. LPCVD silicon can be deposited as masking material. This is an excellent mask even for quite deep etchings.

Regarding borosilicate glass masking is more tricky. The follwing sequence has been used with some success (using sputtered silicon from the Alcatel):

  • Piranha clean
  • Bake-out at 250 C (>2,5 hours)
  • Plasma ashing
  • Sputter-deposit in Alcatel: Power: 550W, Ar-pressure: 10 −2 mbar (base pressure: 10 −6 mbar)
  • Patterning of the silicon using either wet (poly-etch) or dry etching


40% HF 3µm/min Beaker Maske?


Wet HF-etch of bulk glass

Wet Silicon Oxide etch (BHF and SIO Etch (wetting agent)) RIE
General description
  • Isotropic etch
  • Anisotropic etch: vertical sidewalls
Possible masking materials
  • Photoresist
  • Silicon nitride
  • Photoresist
  • (Poly)Silicon
  • Aluminium
  • Chromium (ONLY RIE2!)
  • Other metals that covers less the 5% of the wafer area (ONLY RIE2!)
Etch rate
  • ~75 nm/min (Thermal oxide) in BHF
  • ~90 nm/min (Thermal oxide) in SIO Etch
  • Typically 40-120 nm/min can be increased or decreased by using other recipe parameters.
Uniformity
  • ~ 2% (slow stirring, horizontal wafer)
Batch size
  • 1-25 wafers at a time
  • 1 wafer at a time
Size of substrate
  • 4" wafers
  • 4" wafers or smaller pieces
Allowed materials
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • Blue film
  • Gold (Au) and Nickel (Ni) (but only in BHF2 (KOH)!)
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resist
  • Aluminium
  • Chromium (ONLY RIE2!)
  • Other metals that covers less the 5% of the wafer area (ONLY RIE2!)