Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/DUVetch/polySOI10: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
Created page with "{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;" |+ '''Process runs''' |- ! rowspan="2" width="40"| Date ! colspan="4" width="120"| Substrate Informati..."
 
Jmli (talk | contribs)
No edit summary
Line 15: Line 15:
! width="40" | Wafer ID
! width="40" | Wafer ID
! width="40" | Comments
! width="40" | Comments
|-
! colspan="10" | [[Main Page/Process Logs/jmli/Pegasus/SOI/polySOI10 | Previous runs of this recipe]]
|-
|-
| 28/8-2014
| 28/8-2014

Revision as of 11:43, 2 June 2016

Process runs
Date Substrate Information Process Information SEM Images
Wafer info Mask Material/ Exposed area Tool / Operator Conditioning Recipe Wafer ID Comments
28/8-2014 6" DUVboxA wafer standard stepper mask (50 nm barc + 320 nm krf) Si / 50%+ Pegasus / jmli 30 sec barc etch SOI4\polySOI-10 , 70 cycles or 8:45 minutes S004289

28/8-2014 6" DUVboxB wafer Si/200nm Oxide/1800 nm poly / standard stepper mask (50 nm barc + 320 nm krf) poly / 50%+ Pegasus / jmli 75 sec barc etch SOI4\polySOI-10 , 20 cycles or 2:30 minutes S004289

28/8-2014 6" DUVboxB wafer Si/200nm Oxide/1800 nm poly / standard stepper mask (50 nm barc + 320 nm krf) poly / 50%+ Pegasus / jmli 0 sec barc etch SOI4\polySOI-10 , 30 + 10 cycles or 5:00 minutes S004291 (two processes) S004289 reprocessed, probably overetched -> no spikes