Jump to content

Specific Process Knowledge/Thin film deposition/ALD Picosun R200/ALD multilayers: Difference between revisions

From LabAdviser
Eves (talk | contribs)
Eves (talk | contribs)
Line 213: Line 213:


<gallery caption="" widths="100px" heights="100px" perrow="1">
<gallery caption="" widths="100px" heights="100px" perrow="1">
image:Al2O3_TiO2_flat_multilayers_22.jpg| Al<sub>2</sub>O<sub>3</sub>/TiO<sub>2</sub> multilayers.
image:multilayers222.jpg| Al<sub>2</sub>O<sub>3</sub>/TiO<sub>2</sub> multilayers.
</gallery>
</gallery>



Revision as of 13:34, 20 May 2016

This page describes non standart recipes including multilayers structures.

Low temperature deposition of Al2O3

Recipe: Al2O3 LT

Temperature: 80-150 oC

TMA H2O
Nitrogen flow 150 sccm 200 sccm
Pulse time 0.1 s 0.2 s
Purge time 5.0 s 10.0 s

Deposition rate: 0.089 nm/cycle (@120 oC)

This recipe has been developd for fabrication of high quality homogenious optical layers at low temperature. Research related results with this recipe can be found here: LINK


Al2O3 deposition at 120 oC


Deposition conditions at 120 oC for Al2O3 LT recipe
Number of cycles Thickness (nm) Uniformity across 100mm Si substrate (%) Standard deviation error Refractive index @ 632.8 nm
250 24.83 1.22 0.16 1.61
500 45.48 1.35 0.41 1.63
750 68.03 1.42 0.59 1.63
1000 90.66 1.74 0.94 1.63

%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%


The uniformity, thickness, refractive index has been obtained using Ellipsometer VASE.



Evgeniy Shkondin, DTU Danchip, 2014-2016.

Low temperature deposition of TiO2

Recipe: TiO2 LT

Temperature: 80-150 oC

TiCl4 H2O
Nitrogen flow 150 sccm 200 sccm
Pulse time 0.2 s 0.2 s
Purge time 10.0 s 15.0 s

Deposition rate: 0.048 nm/cycle (@ 120 oC)

This recipe has been developd for fabrication of high quality homogenious optical layers at low temperature. The deposited TiO2 layers are amorphous. Research related results with this recipe can be found here: LINK


TiO2 deposition at 120 oC


Deposition conditions at 120 oC for TiO2 LT recipe
Number of cycles Thickness (nm) Uniformity across 100mm Si substrate (%) Standard deviation error Refractive index @ 632.8 nm
250 10.17 2.19 0.14 2.18
500 23.12 1.80 0.23 2.40
750 34.13 1.87 0.39 2.39
1000 46.13 1.78 0.50 2.39

%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%

The uniformity, thickness, refractive index has been obtained using Ellipsometer VASE.



Evgeniy Shkondin, DTU Danchip, 2014-2016.

Low temperature grown multilayers on flat surfaces

Recipe: EMA01

Recipe: EMA02

Recipe: EMA03

Recipe: EMA04

Temperature: 120 oC


File:Al2O3_TiO2_flat_multilayers.jpg
Evgeniy Shkondin, DTU Danchip, 2014-2016.


Investigation of chemical composition in multilayers system

Chemical taice analysis has been performed using XPS-ThermoScientific equipment in depth profile mode.



Evgeniy Shkondin, DTU Danchip, 2014-2016.

Al2O3/TiO2 multilayers on high aspect ratio structures

Recipe: Multi T

Temperature: 150 oC




Evgeniy Shkondin, DTU Danchip, 2014-2016.