Specific Process Knowledge/Thin film deposition/ALD Picosun R200/ALD multilayers: Difference between revisions
| Line 124: | Line 124: | ||
| align="center" | | | align="center" | | ||
{| border="2" cellspacing="2" cellpadding="3" align="center" style="width:750px" | {| border="2" cellspacing="2" cellpadding="3" align="center" style="width:750px" | ||
! colspan="5" |Deposition conditions at 120 <sup>o</sup>C for | ! colspan="5" |Deposition conditions at 120 <sup>o</sup>C for TiO2 LT recipe | ||
|- | |- | ||
!Number of cycles | !Number of cycles | ||
Revision as of 17:34, 19 May 2016
This page describes non standart recipes including multilayers structures.
Low temperature deposition of Al2O3
Recipe: Al2O3 LT
Temperature: 80-150 oC
| TMA | H2O | |
|---|---|---|
| Nitrogen flow | 150 sccm | 200 sccm |
| Pulse time | 0.1 s | 0.2 s |
| Purge time | 5.0 s | 10.0 s |
Deposition rate: 0.089 nm/cycle (@120 oC)
This recipe has been developd for fabrication of high quality homogenious optical layers at low temperature.
| Al2O3 deposition at 120 oC | |||||||||||||||||||||||||||||||
|
| |||||||||||||||||||||||||||||||
%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%
Low temperature deposition of TiO2
Recipe: TiO2 LT
Temperature: 80-150 oC
| TiCl4 | H2O | |
|---|---|---|
| Nitrogen flow | 150 sccm | 200 sccm |
| Pulse time | 0.2 s | 0.2 s |
| Purge time | 10.0 s | 15.0 s |
This recipe has been developd for fabrication of high quality homogenious optical layers at low temperature. The deposited TiO2 layers are amorphous.
| TiO2 deposition at 120 oC | |||||||||||||||||||||||||||||||
|
| |||||||||||||||||||||||||||||||
%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%% Deposition rate: 0.048 nm/cycle (@ 120 oC)
Low temperature grown multilayers on flat surfaces
Recipe: EMA01
Recipe: EMA02
Recipe: EMA03
Recipe: EMA04
Temperature: 120 oC
Al2O3/TiO2 multilayers on high aspect ratio structures
Recipe: Multi T
Temperature: 150 oC
-
Al2O3/TiO2 multilayers grown on silicon trenches.
Evgeniy Shkondin, DTU Danchip, 2014-2016.