Jump to content

Specific Process Knowledge/Lithography/DUVStepperLithography: Difference between revisions

Taran (talk | contribs)
Taran (talk | contribs)
Line 109: Line 109:


'''Standard processes:'''
'''Standard processes:'''
*'''(1001) DCH 150mm BARC 65nm''' ...
*'''(1001) DCH 150mm BARC 65nm''' Dispense 3ml@1000rpm; spin-off 60s@4700rpm; softbake 60s@175°C
*'''(1002) DCH 100mm BARC 65nm'''
*'''(1002) DCH 100mm BARC 65nm''' Dispense 1.6ml@1000rpm; spin-off 60s@4700rpm; softbake 60s@175°C
*'''(1011) DCH 150mm M230Y 360nm'''
*'''(1011) DCH 150mm M230Y 360nm''' Dispense 3.9ml@1000rpm; spin-off 60s@2500rpm; softbake 90s@130°C
*'''(1012) DCH 100mm M230Y 360nm'''
*'''(1012) DCH 100mm M230Y 360nm''' Dispense 1ml@1000rpm; spin-off 60s@2500rpm; softbake 90s@130°C
*'''(1021) DCH 150mm M35G 750nm'''
*'''(1021) DCH 150mm M35G 750nm'''
*'''(1022) DCH 100mm M35G 750nm'''
*'''(1022) DCH 100mm M35G 750nm'''