==Etching of Titanium==
==Etching of Titanium==
[[Image:Fumehoodetch-chrom2.jpg|300x300px|thumb|Fume hood: positioned in cleanroom 2. <br />Wet Etch of Chromium can take place in a beaker in this fume hood]]
[[Image:Fumehoodetch-chrom2.jpg|300x300px|thumb|Fume hood: positioned in cleanroom 2. <br />Wet Etch of Titanium can take place in this pp tank or in a beaker in this fume hood]]


Etching of Titanium is done wet at Danchip. We have two solutions for titanium etching:
Etching of Titanium is done wet at Danchip. We have two solutions for titanium etching:

Revision as of 11:07, 5 March 2008

Etching of Titanium

Fume hood: positioned in cleanroom 2.
Wet Etch of Titanium can take place in this pp tank or in a beaker in this fume hood

Etching of Titanium is done wet at Danchip. We have two solutions for titanium etching:

  1. BHF
  2. Cold RCA1

Do it by making your own set up in a beaker in a fume hood - preferably in cleanroom 2 or 4. BHF etching can also take place in the PP-etch bath in the fume hood in cleanroom 2.


Comparing the two solutions

BHF Cold RCA1
General description

Etch of titanium with or without photoresist mask.

Etch of titanium (as stripper or with eagle resist).

Chemical solution HF:NH4F NH3OH:H2O2:H2O - 1:1:5
Process temperature Room temperature Room temperature
Possible masking materials

Photoresist (1.5 µm AZ5214E)

Eagle resist

Etch rate

Not known (it bubbles while etching)

Not known

Batch size

1-5 4" in beaker 1-25 wafers at a time in PP-etch bath

1-5 4" wafer at a time

Etch bath Beaker or PP-etch bath in the fume hood in cleanroom 2. Beaker
Allowed materials

No restrictions when used in beaker or PP-etch bath in the fume hood in cleanroom 2. Make a note on the beaker of which materials have been processed.

No restrictions when used in beaker. Make a note on the beaker of which materials have been processed.