SU-8 is an epoxy based negative i-line photoresist with a high contrast. More then 10:1 aspect ratio imaging with vertical sidewalls is one of the widely used properties of this resist. It also has high chemical, plasma and temperature resistance after curing which makes it well suited for permanent use applications. | |||
'''''Note:''' Since the | '''''Note:''' Since the SU-8 is epoxy-based the user is required to take the mandatory epoxy course "Personlig sikkerhed ved arbejde med epoxy". Registration to this course can be found on Portalen under: [http://portalen.dtu.dk/DTU_Generelt/AHR/Ansat/Kompetenceudvikling/Kurser/Arbejdsmiljoe.aspx Arbejdsmiljø kurser] | ||
'' | '' | ||
In Danchip the | In Danchip the SU-8 2000 product line is widely used, where the '''SU-8 2005''' and '''SU-8 2075''' are supplied by Danchip. Other resit formulation can be used but has to be ordered by the user him/herself. | ||
Process recommendations: | Process recommendations: | ||
* a standard process consist of spinning, soft bake, exposure, post bake and development. Please notice that the entire process must be done continuously, meaning that it is not recommendable to spin the resist and then wait until the next day before exposing. | * a standard process consist of spinning, soft bake, exposure, post bake and development. Please notice that the entire process must be done continuously, meaning that it is not recommendable to spin the resist and then wait until the next day before exposing. | ||
* i- line(365nm) radiation is recommended for exposure, therefore use KS or EVG620 aligner, which has i-line filters in the optical system. | * i-line (365nm) radiation is recommended for exposure, therefore use KS or EVG620 aligner, which has i-line filters in the optical system. | ||
* Controlled soft and post bakes are recommended and must be optimized for the specific application, but baseline parameters which can be used as a starting point will be given. | * Controlled soft and post bakes are recommended and must be optimized for the specific application, but baseline parameters which can be used as a starting point will be given. | ||
| Line 19: | Line 19: | ||
==Spinning== | ==Spinning== | ||
SU-8 resist is designed to produce low defect coatings over a very broad range of films thickness. | |||
KS Spinner with RC8 coating module is dedicated to spin all | KS Spinner with RC8 coating module is dedicated to spin all SU-8 resist formulations. | ||
To keep clean room safe and odor free during the spinning please follow the following simple rules: | To keep clean room safe and odor free during the spinning please follow the following simple rules: | ||
| Line 31: | Line 31: | ||
The recommended coating condition: | The recommended coating condition: | ||
* Do manual syringe dispense for the thin resists or use a syringe dispense system for the thick resists. | * Do manual syringe dispense for the thin resists or use a syringe dispense system for the thick resists. | ||
* Do static dispense: approximately 1 ml of | * Do static dispense: approximately 1 ml of SU-8 per inch substrate diameter. | ||
* For | * For SU-8 layers thicker then 100 um use two/step spin coating procedure: | ||
** spread cycle 500rpm, 100rpm/s, 5 sec following by | ** spread cycle 500rpm, 100rpm/s, 5 sec following by | ||
** thickness definition cycle with the final spin speed | ** thickness definition cycle with the final spin speed | ||
** layer uniformity of the thick films can be improved by using a rotation cover(Gyrset), but remember the speed limitation 3000rpm. | ** layer uniformity of the thick films can be improved by using a rotation cover(Gyrset), but remember the speed limitation 3000rpm. | ||
* For | * For SU-8 layers thinner then 10um the spread cycle can be omitted to improve the uniformity of the films. | ||
Here are the spinning curves for SU-8 2002 and SU-8 2005. | Here are the spinning curves for SU-8 2002 and SU-8 2005. | ||
[[media:Spinning_curves.xls|Spinning curves for SU-8 2002 and 2005.]] | [[media:Spinning_curves.xls|Spinning curves for SU-8 2002 and 2005.]] | ||
* A rotation cover(Gyrset) can be also used in case you will spin less then 1um resit | * A rotation cover (Gyrset) can be also used in case you will spin less then 1um resit | ||
** 3000rpm, 300rpm/s, 30sec with gyrset gives appx. 850nm with | ** 3000rpm, 300rpm/s, 30sec with gyrset gives appx. 850nm with SU-8 2002 (the test done by Thomas Buss from Nanotech). | ||
* Another way to get a thinner layer is dilute | * Another way to get a thinner layer is dilute SU-8 2002 in cyclopentanone solution (25ml SU-8 in 80ml cyclopentanone) gives 120nm layer with 7000rpm spinning (the test done by Irene Fernandez-Cuesta and Nimi Gopalakrishnan from Nanotech). | ||
* To achieve a thickness between 80nm and 60nm dilute | * To achieve a thickness between 80nm and 60nm dilute SU-8 2002 in cycopentanone in proportion 5ml SU-8 to 32 ml cyclopentanone. This test is done by Luca Pietrobon from Nanotech. See the spinning curves here.[[media:5ml_SU8_2002_in32ml_cycl.PNG|Diluted SU8 2002.]] | ||
==Baking== | ==Baking== | ||
SU-8 baking can be divided in 2 steps: soft bake step after spinning and post exposure bake after exposure. | |||
The goal of the soft bake step is reducing the amount of solvent in the photoresist layer. The heat application leads to the solvent diffusion to the resist surface and its evaporation. The soft bake step can be done on | The goal of the soft bake step is reducing the amount of solvent in the photoresist layer. The heat application leads to the solvent diffusion to the resist surface and its evaporation. The soft bake step can be done on SU-8 hotplates, marked Hotplates 1 and 2 in LabManager, and usually done in one or two steps with 5-8 deg/min temperature ramp between steps. The soft bake temperature typically is between 20 and 110 C and the soft bake time depends on the film thickness. | ||
The goal of the post exposure bake is increasing the polymerization reaction even the polymerization can in principle take place at room temperature. The post exposure step can be done at the same hotplates, as the soft bake step, with the temperature range between 20 and 120C and with temperature ramping 5-8 deg/min. | The goal of the post exposure bake is increasing the polymerization reaction even the polymerization can in principle take place at room temperature. The post exposure step can be done at the same hotplates, as the soft bake step, with the temperature range between 20 and 120C and with temperature ramping 5-8 deg/min. | ||
| Line 59: | Line 59: | ||
The exposure step is usually done in near UV-radiation at aligners system which has i-line filter (365nm wavelength). At Danchip we have 2 aligners which can be used for this: KS Aligner or EVG620. | The exposure step is usually done in near UV-radiation at aligners system which has i-line filter (365nm wavelength). At Danchip we have 2 aligners which can be used for this: KS Aligner or EVG620. | ||
Duration of the UV-exposure depends of resist thickness, but notice that if the UV exposure becomes long then the heating at the interface with the mask can cause formation of hard skin at the surface of | Duration of the UV-exposure depends of resist thickness, but notice that if the UV exposure becomes long then the heating at the interface with the mask can cause formation of hard skin at the surface of SU-8 so called T-topping phenomena. The the main rule is if the dose of the exposure exceeds 250-300 mJ/cm2 it is recommended to do a multiple exposure instead and have a waiting time between the steps to allow the resist cool down. | ||
==Developing== | ==Developing== | ||
Developing of the | Developing of the SU-8 patterns is done in the special developing station placed in CR3 at Danchip. Under developing the substrates are immersed in Propylene Glycol Methyl Ether Acetate (PGMEA) first in a bath marked "First" and after in a bath marked "Final". | ||
The development time is dependent on the layer thickness. | The development time is dependent on the layer thickness. | ||
After the development the substrate must be rinsed with Isopropyl Alcohol(IPA)on both side for 30 sec. White traces during rinsing indicate incomplete development of | After the development the substrate must be rinsed with Isopropyl Alcohol (IPA) on both side for 30 sec. White traces during rinsing indicate incomplete development of SU-8. | ||
Finally the substrates are dried in air in the drying box or with a nitrogen gun. | Finally the substrates are dried in air in the drying box or with a nitrogen gun. | ||
Revision as of 10:55, 7 April 2016
SU-8 is an epoxy based negative i-line photoresist with a high contrast. More then 10:1 aspect ratio imaging with vertical sidewalls is one of the widely used properties of this resist. It also has high chemical, plasma and temperature resistance after curing which makes it well suited for permanent use applications.
Note: Since the SU-8 is epoxy-based the user is required to take the mandatory epoxy course "Personlig sikkerhed ved arbejde med epoxy". Registration to this course can be found on Portalen under: Arbejdsmiljø kurser
In Danchip the SU-8 2000 product line is widely used, where the SU-8 2005 and SU-8 2075 are supplied by Danchip. Other resit formulation can be used but has to be ordered by the user him/herself.
Process recommendations:
- a standard process consist of spinning, soft bake, exposure, post bake and development. Please notice that the entire process must be done continuously, meaning that it is not recommendable to spin the resist and then wait until the next day before exposing.
- i-line (365nm) radiation is recommended for exposure, therefore use KS or EVG620 aligner, which has i-line filters in the optical system.
- Controlled soft and post bakes are recommended and must be optimized for the specific application, but baseline parameters which can be used as a starting point will be given.
Pretreatment
- To dehydrate the surface, bake in 250C oven at least 30 min, the longer the bake the better. Baking overnight is recommended.
- Another dehydration step can be done in the HMDS oven using recipe 9. This does not expose the wafers to HMDS but instead makes a bakeout at reduced pressure
Spinning
SU-8 resist is designed to produce low defect coatings over a very broad range of films thickness.
KS Spinner with RC8 coating module is dedicated to spin all SU-8 resist formulations.
To keep clean room safe and odor free during the spinning please follow the following simple rules:
- Always use point exhaust above the place you handle the resist.
- To minimize fumes of resist keep the wafers with resist in the extract box prior the baking.

- When you move the wafers to the dedicated hot plates always carry them in a close container.
The recommended coating condition:
- Do manual syringe dispense for the thin resists or use a syringe dispense system for the thick resists.
- Do static dispense: approximately 1 ml of SU-8 per inch substrate diameter.
- For SU-8 layers thicker then 100 um use two/step spin coating procedure:
- spread cycle 500rpm, 100rpm/s, 5 sec following by
- thickness definition cycle with the final spin speed
- layer uniformity of the thick films can be improved by using a rotation cover(Gyrset), but remember the speed limitation 3000rpm.
- For SU-8 layers thinner then 10um the spread cycle can be omitted to improve the uniformity of the films.
Here are the spinning curves for SU-8 2002 and SU-8 2005. Spinning curves for SU-8 2002 and 2005.
- A rotation cover (Gyrset) can be also used in case you will spin less then 1um resit
- 3000rpm, 300rpm/s, 30sec with gyrset gives appx. 850nm with SU-8 2002 (the test done by Thomas Buss from Nanotech).
- Another way to get a thinner layer is dilute SU-8 2002 in cyclopentanone solution (25ml SU-8 in 80ml cyclopentanone) gives 120nm layer with 7000rpm spinning (the test done by Irene Fernandez-Cuesta and Nimi Gopalakrishnan from Nanotech).
- To achieve a thickness between 80nm and 60nm dilute SU-8 2002 in cycopentanone in proportion 5ml SU-8 to 32 ml cyclopentanone. This test is done by Luca Pietrobon from Nanotech. See the spinning curves here.Diluted SU8 2002.
Baking
SU-8 baking can be divided in 2 steps: soft bake step after spinning and post exposure bake after exposure.
The goal of the soft bake step is reducing the amount of solvent in the photoresist layer. The heat application leads to the solvent diffusion to the resist surface and its evaporation. The soft bake step can be done on SU-8 hotplates, marked Hotplates 1 and 2 in LabManager, and usually done in one or two steps with 5-8 deg/min temperature ramp between steps. The soft bake temperature typically is between 20 and 110 C and the soft bake time depends on the film thickness.
The goal of the post exposure bake is increasing the polymerization reaction even the polymerization can in principle take place at room temperature. The post exposure step can be done at the same hotplates, as the soft bake step, with the temperature range between 20 and 120C and with temperature ramping 5-8 deg/min. It is important to do the post exposure bake immediately after exposure to limit photoinitiator diffusion into non-exposed areas.
Exposure
The exposure step is usually done in near UV-radiation at aligners system which has i-line filter (365nm wavelength). At Danchip we have 2 aligners which can be used for this: KS Aligner or EVG620.
Duration of the UV-exposure depends of resist thickness, but notice that if the UV exposure becomes long then the heating at the interface with the mask can cause formation of hard skin at the surface of SU-8 so called T-topping phenomena. The the main rule is if the dose of the exposure exceeds 250-300 mJ/cm2 it is recommended to do a multiple exposure instead and have a waiting time between the steps to allow the resist cool down.
Developing
Developing of the SU-8 patterns is done in the special developing station placed in CR3 at Danchip. Under developing the substrates are immersed in Propylene Glycol Methyl Ether Acetate (PGMEA) first in a bath marked "First" and after in a bath marked "Final".
The development time is dependent on the layer thickness.
After the development the substrate must be rinsed with Isopropyl Alcohol (IPA) on both side for 30 sec. White traces during rinsing indicate incomplete development of SU-8.