Specific Process Knowledge/Thin film deposition/Deposition of Titanium: Difference between revisions
| Line 193: | Line 193: | ||
== Comments: Choise of equipment == | == Comments: Choise of equipment == | ||
'''Thick layers''' | |||
Practical experience has shown that at some occation it is better to use the Wordentec than the Alcatel for thicker Ti layers. Deposition of 5000 Å Ti on Si is working fine in both machines. However, with the same thickness of Ti deposited on pyrex+resist, the metal layer deposited in Alcatel may have metal flakes in the center of the wafer. The process workes without problems in Wordentec. | |||
== Comments: Adhesion layer == | == Comments: Adhesion layer == | ||
Revision as of 17:32, 4 March 2016
Feedback to this page: click here
Titanium deposition
Titanium can be deposited by e-beam evaporation. In the chart below you can compare the different deposition equipment.
| E-beam evaporation (Alcatel) | E-beam evaporation (Wordentec) | E-beam evaporation (PVD co-sputter/evaporation) | E-beam evaporation (Physimeca) | Sputter deposition (Wordentec) | Sputter deposition (Lesker) | E-beam evaporation (III-V Dielectric evaporator) | |
|---|---|---|---|---|---|---|---|
| General description | E-beam deposition of Titanium | E-beam deposition of Titanium | E-beam deposition of Titanium | E-beam deposition of Titanium | Sputter deposition of Titanium | Sputter deposition of Titanium | E-beam deposition of Titanium |
| Pre-clean | RF Ar clean | RF Ar clean | RF Ar clean | RF Ar clean | RF Ar clean | ||
| Layer thickness | 10Å to 1µm* | 10Å to 1 µm* | 10Å to 2000Å | 10Å to 1000Å | . | . | 10Å to 1000Å |
| Deposition rate | 2Å/s to 15Å/s | 10Å/s to 15Å/s | About 1Å/s | About 10Å/s | Depending on process parameters, see here. | Depending on process parameters, about 1 Å/s. | About 1Å/s |
| Batch size |
|
|
|
|
|
|
|
| Allowed substrates |
|
|
|
|
|
|
|
| Allowed materials |
|
|
|
|
|
|
|
| Comment | Only very thin layers (up to 100nm). |
* For thicknesses above 200 nm permission from ThinFilm group (thinfilm@danchip.dtu.dk) is required.
Comments: Choise of equipment
Thick layers
Practical experience has shown that at some occation it is better to use the Wordentec than the Alcatel for thicker Ti layers. Deposition of 5000 Å Ti on Si is working fine in both machines. However, with the same thickness of Ti deposited on pyrex+resist, the metal layer deposited in Alcatel may have metal flakes in the center of the wafer. The process workes without problems in Wordentec.
Comments: Adhesion layer
Ti as adhesion layer
Titanium is most often used as a adhesion layer for other metals, like for example gold. Gold does not stick very well to Si, and to prevent it to come off in future process steps or in the final application, a layer of Ti (or Cr) is often deposited onto the wafer.
The most common thickness of the Ti adhesion layer is 10 nm. Also layers with a thickness of 5 nm is used.
Very thin adhesion layers
If it is important to have a very thin Ti layer, it is possible to use even thinner adhesion layers. There are some experiences of using a 3 nm Ti as adhesion layer for a 200 nm thick gold layer. In this case a Si wafer was dipped in buffer and rinsed in water immediately before being placed in the PVD equipment (Wordentec). After a RF clean process of the wafer, 3nm of Ti and 200 nm of Au was deposited, and this worked fine during futher processing.